Bronze and Wear-Resistant Grade Selection for Three Rolling Mill Components
Bronze and Wear-Resistant Grade Selection for Three Rolling Mill Components
High-Performance Self-Lubricating Bronze Bushing Solutions & Technologies. Minimize downtime, extend service life, and reduce costs for dynamic applications.
Bronze and Wear-Resistant Grade Selection for Three Rolling Mill Components
Tin bronze slide plate, aluminium bronze bushing and high manganese steel wear plate — composition, mechanical properties, dimensional requirements and acceptance items
Scope. Three wear components in rolling mill equipment are specified below with their technical conditions. Two are copper alloys accepted under one standard; the third belongs to a separate material system and is accepted independently. The purpose of this document is to state the composition limits, mechanical property minima, dimensional requirements and acceptance items for each position, and to record the verification findings that affect specification writing.
Contents
- Component summary and material system assignment
- Slide plate — ZCuSn10Pb5, cast tin bronze
- Bushing — ZCuAl10Fe3, cast aluminium bronze
- Wear plate — ZGMn13Cr2, high manganese cast steel
- Pairing relationship and hardness differential
- Acceptance items by component
- Verification findings
- Items requiring confirmation
- Alternative grade routes
- Frequently asked questions
1. Component summary and material system assignment
| Component | Designation | Material system | Governing standard | Selection role | Governing limit |
|---|---|---|---|---|---|
| Slide plate | ZCuSn10Pb5 | Copper alloy cast tin bronze |
GB/T 1176-2013 item 6 |
Low speed reciprocating; anti-seizure |
Allowable continuous temperature 200 °C. Contains lead; not for potable water or food contact. Above approximately 20 MPa contact pressure a change of grade is indicated. |
| Bushing | ZCuAl10Fe3 | Copper alloy cast aluminium bronze |
GB/T 1176-2013 item 21 |
Heavy load low speed; compressive capacity |
Dry operation without lubricant is not admissible. The alloy has no free-lead self-lubricating phase and depends on a continuous oil supply. |
| Wear plate | ZGMn13Cr2 | Cast steel wear part not a copper alloy |
GB/T 24186 GB/T 5680 series |
High impact; work hardening |
Water toughening is a mandatory process step. In low-stress sliding or erosion duty the work-hardening mechanism does not activate. |
Material system assignment. ZGMn13Cr2 is a high manganese cast steel wear part specified under GB/T 24186 and the GB/T 5680 series. It is not a copper alloy and does not fall under GB/T 1176. Accepting the wear plate against the copper alloy standard would place it in the wrong material system. The slide plate and bushing are both copper alloys and may be accepted under the same standard, listed separately. The wear plate is accepted independently.
2. Slide plate — ZCuSn10Pb5, cast tin bronze
2.1 Composition (GB/T 1176-2013, item 6)
| Element | Specified limit | Function or control point |
|---|---|---|
| Designation | ZCuSn10Pb5 / tin bronze 10-5 | Former designation ZQSn10-5 |
| Alloy system | Cu-Sn-Pb ternary | Lead-bearing grade. Tin solid solution matrix with discrete free-lead particles |
| Sn | 9.0 – 11.0 % | Solution strengthening of the matrix; establishes strength and hardness |
| Pb | 4.0 – 6.0 % | Discrete soft particles that form a transferred lubricant film at the sliding surface |
| Zn | ≤ 1.0 % | Melt fluidity; excluded from the impurity total |
| Fe / Sb | ≤ 0.3 % / ≤ 0.3 % | Controlled to prevent hard inclusions scoring the mating surface |
| P | ≤ 0.05 % | Low-phosphorus grade. Fatigue strength below that of ZCuSn10P1 |
| Al / Si | ≤ 0.02 % / ≤ 0.02 % | Controlled to avoid brittle inclusions affecting casting soundness |
| Total impurities | ≤ 1.0 % | Cu balance |
2.2 Mechanical properties by casting method
| Casting method | Tensile Rm | Elongation A | Hardness HBW | Selection note |
|---|---|---|---|---|
| Sand cast S | ≥ 195 MPa | ≥ 10 % | ≥ 70 | Large or complex shapes; lower strength |
| Metal mould J | ≥ 245 MPa | ≥ 10 % | ≥ 70 | Specified where conformity of the sliding face is required |
| Centrifugal Li | Denser structure; values above metal mould | — | — | Improves lead phase distribution |
Governing limits. Density approximately 8.9 g/cm³, coefficient of thermal expansion approximately 18.4 × 10⁻⁶/K, elastic modulus approximately 100 GPa.
- Allowable continuous temperature 180 °C, short-time peak 200 °C. Above this range the lead phase segregates and both lubrication and wear resistance decline.
- The phosphorus content is low, so fatigue strength is below ZCuSn10P1; the grade is not suited to continuous high-speed alternating loading.
- Prolonged dry sliding accelerates wear. A base oil film is required.
- Lead-bearing: not for potable water or food contact service. Lead-free export projects require a different grade.
2.3 Suitability assessment
| Duty characteristic | Behaviour of ZCuSn10Pb5 | Assessment |
|---|---|---|
| Low speed reciprocating sliding | Good conformability; conforms under micro-movement | Suited Typical slide plate duty |
| Anti-seizure / seizure prevention | Free-lead particles form a lubricant film; stable friction behaviour | Suited Above lead-free tin bronze |
| Oxide scale contamination | Soft lead particles embed hard debris, protecting the mating steel | Suited Embeddability above ZCuSn10P1 |
| High contact pressure | Sand cast Rm only ≥195 MPa; limited compressive capacity | Marginal Above approximately 20 MPa, aluminium bronze is indicated |
| High speed continuous sliding | Lead phase has limited resistance to being washed out | Not suited Change to tin bronze or aluminium bronze |
| Above 200 °C | Lead phase ceases to function | Not suited Grade change required |
2.4 International designation cross-reference
| Region | Designation | Note |
|---|---|---|
| China GB/T 1176 | ZCuSn10Pb5 | Reference designation |
| United States UNS | C92710 | Related designation; no exact equivalent |
| Europe EN 1982 | CC484K / G-CuSn10Pb5 | Material number 2.1170; composition range differs slightly from the GB designation |
| Japan JIS | BC2C / LBC2 | Related designation |
| ISO 1338 | CuSn10Pb | Corresponding designation |
Export note. This grade is not C93700 and is not C90700. C93700 specifies lead at 8–11 %, giving stronger self-lubrication at the expense of matrix strength. ZCuSn10Pb5 has higher tin and lower lead, so the matrix is stiffer and dimensional stability is better suited to a precision slide plate. Designations are not interchangeable across specifications without checking each composition range.
3. Bushing — ZCuAl10Fe3, cast aluminium bronze
Selection role. Of the three components, the aluminium bronze offers the highest compressive load capacity of the copper alloys (sand cast Rm ≥490 MPa; metal mould and centrifugal ≥540 MPa). For a bushing this is the conventional heavy-duty arrangement in rolling mill copper practice. The selection logic is the reverse of the slide plate: the slide plate is chosen for softness and conformability, the bushing for hardness and compressive resistance.
3.1 Composition (GB/T 1176-2013, item 21)
| Element | Specified limit | Function or control point |
|---|---|---|
| Designation | ZCuAl10Fe3 / aluminium bronze 10-3 | Former designation ZQAl9-4 |
| Alloy system | Cu-Al-Fe | Lead-free and nickel-free; cost below nickel aluminium bronze |
| Al | 8.5 – 11.0 % | Solution strengthening; forms a protective aluminium oxide film |
| Fe | 2.0 – 4.0 % | Forms κ (FeAl) hard phase; grain refinement and wear resistance |
| Ni | ≤ 3.0 % | Excluded from the impurity total. Permitted by GB; nickel aluminium bronze is specified instead for seawater duty |
| Mn | ≤ 1.0 % | Excluded from the impurity total. Supplementary toughness |
| Zn | ≤ 0.4 % | Zinc-free formulation, so dezincification does not arise |
| Sn / Pb / Si | ≤ 0.3 % / ≤ 0.2 % / ≤ 0.2 % | Controlled impurities |
| Total impurities | ≤ 1.0 % | Cu balance |
3.2 Mechanical properties by casting method
| Casting method | Tensile Rm | Yield Rp0.2 | Elongation A | Hardness HBW | Application |
|---|---|---|---|---|---|
| Sand cast S | ≥ 490 MPa | ≥ 180 MPa | ≥ 13 % | ≥ 100 | Large sections |
| Metal mould J | ≥ 540 MPa | ≥ 200 MPa | ≥ 15 % | ≥ 110 | Complex shapes |
| Centrifugal Li | ≥ 540 MPa | ≥ 200 MPa | ≥ 15 % | ≥ 110 | Specified for bushings |
Data correction. A number of technical pages report the hardness of this grade as “980 HB”, “1080 HB” or “980–1080 HB”. These figures are tensile strength values in MPa, not Brinell hardness.
The specified hardness values are: sand cast ≥100 HBW; metal mould, continuous and centrifugal ≥110 HBW. Acceptance should be written in HBW. If a supplier material certificate shows a hardness value in the region of 980 HB or above, the entry should be treated as a data error and corrected before acceptance.
3.3 Physical properties and process parameters
| Parameter | Value, as-cast | Engineering implication |
|---|---|---|
| Density | 7.45 – 7.8 g/cm³ | Approximately three quarters that of steel; lower inertia loading |
| Elastic modulus | 110 – 118 GPa | Lower stiffness than steel; greater deflection under load, so clearance must absorb it |
| Coefficient of thermal expansion | 16.6 – 17.8 × 10⁻⁶/K | Higher than steel (approximately 11 × 10⁻⁶/K), so clearance must be increased for elevated temperature duty |
| Thermal conductivity | 41 – 58 W/(m·K) | Above tin bronze; carries frictional heat away more effectively |
| Solidus / liquidus | 1030 °C / 1080 °C | Pouring at 1100–1180 °C; melting and heating temperature 1200–1250 °C |
| Allowable continuous temperature | ≤ 250 °C (short-time peak ≤280 °C) | Above 300 °C the matrix loses strength |
3.4 Bushing structural and machining requirements
| Item | Specified value or method | Reason |
|---|---|---|
| Casting process | Centrifugal casting specified | The alloy solidifies in a mushy range; sand cast thick sections are prone to intergranular shrinkage. Centrifugal castings show a denser structure and markedly less porosity |
| Melt practice | Pre-mastered Al-Fe intermediate alloy | Balances the melting point difference between aluminium and iron: melt copper, then add return material and intermediate alloy, then clean and adjust to pouring temperature |
| Wall thickness | ≥ 0.08 – 0.10 × journal diameter | Example: a 60 mm bore requires 5–6 mm wall. An alternative form is t = 0.05 × ID + (2 to 6) mm |
| Length to diameter ratio | L/ID = 0.5 – 2.0 | Values below 1 are used for high load or high speed, reducing misalignment, edge loading and heat generation |
| Running clearance | 0.1 – 0.2 % of shaft diameter | Aluminium bronze expands further than steel, so clearance should exceed the tin bronze value. Lower end for heavy low-speed duty, upper end for high-speed or elevated-temperature duty |
| Interference, OD to housing | 0.05 – 0.12 % of OD | Too little permits microslip wear; too much makes pressing difficult and may be lost after the housing yields |
| Bore lead-in | 1 – 2 mm chamfer, polished | Prevents the bushing bore being scored during pressing |
| Oil grooves | Circumferential and axial grooves required | Grooves are placed in the unloaded half of the bore. A groove on the load line removes load-carrying area where stress is highest |
| Debris grooves | Required | Clears oxide scale particles and limits three-body abrasion |
| Bore roughness | Ra 0.8 – 1.6 μm | Below 0.4 μm the surface lacks oil retention structure; above 3.2 μm asperities rupture the lubricant film |
| Journal finish | Ra 0.4 – 0.8 μm, ground | A ground journal typically gives about twice the bearing life of a turned surface |
| Heat treatment | 260 – 320 °C stress relief | Applied before finish machining to relieve casting stress and prevent distortion. The alloy cannot be extruded or forged |
| Heavy thick sections | 700 °C soak followed by air cooling | Avoids brittle structure from slow cooling |
| Weld repair | TIG, preheat 200–300 °C | The grade is weldable for defect repair; not suited to brazing. Cool slowly after welding and relieve stress |
| Machining | Carbide tooling, ample coolant | Machinability is moderate and toughness high, so cutting forces exceed those for tin bronze. Bore by boring and honing |
3.5 Suitability assessment
| Duty characteristic | Behaviour of ZCuAl10Fe3 | Assessment |
|---|---|---|
| High contact pressure | Compressive strength well above tin bronze and brass; resists flattening under high pressure | Suited Principal advantage at this position |
| Heavy load with shock | α matrix with κ hard phase; resists cracking under impact | Suited Clearly above tin bronze |
| Oil-lubricated anti-seizure | κ hard particles form a wear skeleton resisting scoring | Suited Requires a reliable oil supply |
| Fresh water / atmospheric | Aluminium oxide film; zinc-free formulation | Suited Above ordinary brass |
| Dry sliding without lubricant | No free-lead self-lubricating phase | Not suited Prolonged dry operation is not admissible; embed solid lubricant or guarantee oil supply |
| Seawater immersion / cavitation | No nickel or manganese; limited pitting and cavitation resistance; prone to dealuminification | Not suited Specify nickel aluminium bronze |
| Very high rotational speed | Grade positioned for low and medium speed | Marginal Specify tin bronze at high speed |
| Heat treatment strengthening | No precipitation hardening capability; quenching and ageing give limited gain | The 700 °C air cool serves only to reduce brittleness in castings |
3.6 International designation cross-reference
| Region | Designation | Note |
|---|---|---|
| China GB/T 1176 | ZCuAl10Fe3 | Reference designation, item 21 |
| United States UNS | C95400 | Related designation (C95200 also related) |
| Europe EN 1982 | CC331G / CuAl10Fe2-C | EN 2.0940 |
| Japan JIS H5120 | CAC702 | ALBC2 |
| United Kingdom BS 1400 | AB1 | — |
Designation mapping caution. EN 1982 CC333G is not the counterpart of C95400. CC333G is the cast nickel aluminium bronze CuAl10Fe5Ni5-C, corresponding to the C95500 and C95800 group. The iron-bearing C95400 corresponds to CC331G (CuAl10Fe2-C). It is also worth noting that C95500 is supplied heat-treatable because of its nickel content, whereas C95400 is used in the as-cast condition. The two are not the same alloy at different nickel contents.
4. Wear plate — ZGMn13Cr2, high manganese cast steel
Material system. This designation is a cast steel wear part specified under GB/T 24186 and the GB/T 5680 series. It is not a copper alloy and GB/T 1176 does not apply. In a purchase document it should be listed as a separate material item, accepted independently of the slide plate and bushing.
4.1 Composition and mechanical properties
| Item | Value or range | Function or control point |
|---|---|---|
| C | 1.0 – 1.4 % | Work-hardening potential and carbide source; excessive carbon precipitates brittle grain boundary carbides |
| Mn | 11.0 – 14.0 % | Stabilises the austenitic matrix and provides toughness — the basis of the designation |
| Cr | 1.5 – 2.5 % | Grain refinement, suppression of continuous network carbides, higher initial hardness and corrosion resistance |
| Si | 0.6 – 1.0 % | Deoxidation |
| P / S | ≤ 0.04 % / ≤ 0.04 % | Controlled impurities; lower values give higher toughness |
| Hardness, water toughened | HB 180 – 240 | Acceptance reference condition. Initially soft; hardening requires impact loading |
| Hardness after work hardening | HB 500 – 550+ | Hardened layer typically 1–5 mm deep; the core retains toughness |
| Tensile strength | ≥ 735 – 880 MPa | — |
| Impact toughness | ≥ 100 – 150 J/cm² | Hard surface with a tough core; absorbs energy without fracture |
| International | ASTM A128 | Corresponding United States designation for high manganese castings |
4.2 Water toughening — mandatory process
As-cast parts must not be installed without water toughening. In the as-cast condition the grain boundaries of high manganese steel are filled with brittle continuous carbides, and light impact may cause fracture. The process sequence is:
- Heat gradually in stages to 680 °C to relieve casting stress (80–100 °C/h, hold about 1.5 h), preventing thermal cracking in thick sections.
- Continue to 1050–1100 °C (about 120 °C/h) and hold according to wall thickness: 2–2.5 h at ≤50 mm, 3–4 h at 50–100 mm, so that carbides dissolve fully into the austenite.
- Transfer to circulating water at ≤30 °C within 30 seconds of leaving the furnace (water volume at least ten times the total part weight), cooling rate ≥30 °C/s.
- Air cool naturally after removal. Do not temper or slow cool.
Embrittlement range. Holding between 250 °C and 500 °C reprecipitates grain boundary carbides, and toughness falls sharply with cracking. Process control is required if the component passes through that range.
4.3 Selection boundary
Where the grade applies: high impact and extrusion
The austenitic surface hardens by deformation under impact and extrusion, rising from approximately HB 200 to above HB 500. As one layer wears away, the newly exposed surface hardens again.
Typical positions: high impact stress areas in rolling mills, and liners in crushing equipment subject to large lump impact.
Where the grade does not apply: low-stress sliding
Work hardening does not activate under pure sliding or erosion duty. In that condition the wear resistance is lower than that of hardness-controlled materials such as high chromium cast iron.
Specifying this grade for a position dominated by continuous water erosion on a rolling mill is a selection error.
| Duty characteristic | Assessment | Note |
|---|---|---|
| High impact with strong extrusion (rolling load, bite-in) | Applicable | Work hardening is fully activated; this is the primary duty for the grade |
| Medium impact with medium abrasive wear | Applicable | Chromium content slows early wear; service life exceeds plain Mn13 |
| Low-stress sliding or erosion without impact | Not applicable | Hardening does not activate. Specify high chromium cast iron (GB/T 3226 series) or an AR-grade low alloy wear steel instead |
| Sustained operation above 300 °C | Not applicable | Structure changes; specify a heat-resistant wear material |
| Weld repair | Restricted | Weldability is poor. Preheat to avoid cracking and control heat input to stay out of the 250–500 °C embrittlement range. Significant load-bearing welds should be re-water toughened |
5. Pairing relationship and hardness differential
The bushing and slide plate form a typical sliding pair. The bushing (ZCuAl10Fe3, HBW ≥110) is harder than the slide plate (ZCuSn10Pb5, HBW ≥70). The gradient direction is correct: the softer member carries the wear, so replacing the slide plate is lower cost than replacing the bushing.
It must be confirmed that the steel journal or rail is harder than both components. Where the copper part is not the softer element, it ceases to function as a sacrificial wear element and becomes the damage source.
| Component | Designation | Hardness HBW | Role in the pair | Check item |
|---|---|---|---|---|
| Slide plate | ZCuSn10Pb5 | ≥ 70 | Softer side; carries wear | Should be softer than the bushing and the mating steel |
| Bushing | ZCuAl10Fe3 | ≥ 110 | Harder side; carries the load | Harder than the slide plate, softer than the steel journal |
| Steel journal or rail | Steel (purchaser specified) | Highest of the three | Datum component; must not be scored | Hardness data to be provided by the purchaser, otherwise the gradient cannot be verified |
6. Acceptance items by component
Slide plate — ZCuSn10Pb5
- Designation and standard: ZCuSn10Pb5, GB/T 1176-2013, with the casting method stated (metal mould J specified)
- Hardness accepted as HBW ≥ 70, with sampling position and test method stated
- Sliding surface roughness Ra 1.6–3.2 μm; mounting face flatness within 0.05 mm
- Oil groove form (herringbone, cross or diamond) and debris groove layout — oxide scale must be able to escape
- Confirm the working temperature does not exceed 200 °C
- Lead compliance declaration: export projects to state that the grade is not used for potable water or food contact
- Confirm contact pressure: above approximately 20 MPa, reassess whether aluminium bronze is indicated
Bushing — ZCuAl10Fe3
- Designation and standard: ZCuAl10Fe3, GB/T 1176-2013, with centrifugal casting specified
- Hardness accepted as HBW ≥ 110 for centrifugal or metal mould, ≥ 100 for sand casting. A certificate showing a value in the region of 980 HB is a data error
- Wall thickness ≥ 0.08–0.10 × journal diameter; journal diameter to be provided so this can be checked
- Running clearance calculated at 0.1–0.2 % of shaft diameter and entered on the drawing; increased for elevated-temperature duty
- Interference, bore lead-in chamfer 1–2 mm, and oil groove position clear of the load-carrying area
- Confirm lubrication is by oil supply. For unlubricated duty the component must be changed to a solid-lubricant-embedded structure or to a different grade
- Record of stress relief at 260–320 °C; 700 °C air cool for heavy thick sections
- UT or MT inspection advised for load-bearing parts, with the acceptance criterion stated in the contract
- Confirm the environment is not continuous seawater immersion. If it is, specify nickel aluminium bronze
Wear plate — ZGMn13Cr2
- State GB/T 24186 or GB/T 5680 as the standard. Do not reference a copper alloy standard
- Chemical composition: C, Mn and Cr are the principal acceptance elements; P and S are upper limits
- Water toughening is a mandatory acceptance item. Delivered hardness should be in the water toughened range HB 180–240. Hardness above that range indicates an embrittlement risk rather than a better product
- Impact toughness ≥100 J/cm² where the drawing requires it
- Surface quality: no cracks or cold shuts; gating, risers, adhering sand and flash removed
- Inspection: UT or MT advised for heavy sections, with the acceptance criterion stated in the contract
- Confirm that the position is genuinely an impact duty. For pure sliding or erosion, the grade should be changed
- Mounting faces free of cracks; cutting and welding operations kept out of the 250–500 °C embrittlement range
7. Verification findings
| No. | Item checked | Result | Action |
|---|---|---|---|
| 1 | ZCuSn10Pb5 status in GB/T 1176-2013 | Present, item 6, tin bronze 10-5 | Designation valid; may be referenced directly |
| 2 | Phosphorus content of ZCuSn10Pb5 | ≤ 0.05 %, a low-phosphorus grade, materially different from ZCuSn10P1 (0.8–1.1 %) | Fatigue strength is below the P1 grade; verify at delivery |
| 3 | Hardness of ZCuSn10Pb5 | Specified value HBW ≥ 70; no mislabelling found | Accept against HBW 70 |
| 4 | Relationship to C93700 | Different lead content (4–6 % against 8–11 %); strength and lubrication priorities oppose each other | Not interchangeable. State the designation on the contract |
| 5 | ZCuAl10Fe3 hardness mislabelled | Several pages report “980 HB” or “1080 HB” — these are tensile strength values in MPa | Correct values: sand cast ≥100 HBW, centrifugal ≥110 HBW. Added to acceptance items |
| 6 | EN designation for ZCuAl10Fe3 | Should be CC331G (CuAl10Fe2-C), not CC333G | CC333G is CuAl10Fe5Ni5-C, the nickel-bearing grade |
| 7 | Corrosion limitation of ZCuAl10Fe3 | No nickel or manganese; not suited to continuous seawater immersion or cavitation | Specify nickel aluminium bronze for seawater duty |
| 8 | Heat treatment capability of ZCuAl10Fe3 | No precipitation hardening capability; quenching and ageing give limited gain | The 700 °C air cool serves only to reduce casting brittleness |
| 9 | Wall thickness and clearance values | Several sources differ; general engineering values adopted with the basis stated | Wall ≥0.08–0.10 × D; clearance 0.1–0.2 % × D; both entered on the drawing |
| 10 | Material system of ZGMn13Cr2 | Cast steel wear part, not a copper alloy | List separately; accept independently of the copper parts |
| 11 | Hardness range of ZGMn13Cr2 | Sources give HB 170–220, 180–240 and 200–250 | Adopted HB 180–240 in the water toughened condition as the reference, with the condition stated |
| 12 | Applicable duty for ZGMn13Cr2 | High impact duty; not valid for low-stress sliding | Duty description attached to the contract to avoid misuse on erosion positions |
| 13 | Carbon content of ZGMn13Cr2 | Two forms appear: C 0.90–1.30 and C 1.0–1.4 | The cited edition of GB/T 24186 governs; state the standard and year on the contract |
8. Items requiring confirmation
| Priority | Component | To be confirmed | Effect on selection |
|---|---|---|---|
| High | Bushing | Journal diameter, working temperature and mating steel hardness | Determines whether wall thickness, running clearance and the hardness gradient can be calculated and verified |
| High | Bushing | Whether lubrication is by oil supply | The grade has no self-lubricating phase. Without oil, the component must change to an embedded solid-lubricant structure or to a different grade |
| High | Wear plate | Whether the position is impact dominated or erosion dominated | For pure sliding or erosion, ZGMn13Cr2 is a selection error |
| High | Slide plate | Whether the working temperature exceeds 200 °C | Above that value the lead phase ceases to function and the grade must change |
| High | Slide plate | Actual contact pressure in MPa | Above approximately 20 MPa, aluminium bronze is indicated |
| Medium | Bushing | Whether the environment is seawater or continuous water erosion | Seawater indicates nickel aluminium bronze; erosion raises dry-friction risk |
| Medium | Wear plate | Whether impact toughness and inspection level are required | Determines the acceptance items and whether UT or MT is added |
| Medium | Slide plate | Environmental and lead-free requirements for the export project | A lead-bearing grade requires a stated exemption, or a lead-free route |
| Low | All | Whether all components are supplied by one supplier | Affects contract structure and allocation of responsibility |
9. Alternative grade routes
| Component | Condition | Alternative grade |
|---|---|---|
| Bushing | Calculated contact pressure exceeds the compressive capacity of aluminium bronze, or a higher yield strength is required | Nickel aluminium bronze ZCuAl10Ni5Fe4 — heat treatable, higher yield strength. Also the route for seawater and cavitation duty |
| Slide plate | Contact pressure above approximately 20 MPa, or the export project requires lead-free material | Aluminium bronze ZCuAl10Fe3 (higher compressive and temperature capacity, with lower anti-seizure behaviour, so good lubrication is required) or tin bronze ZCuSn10P1 (lead-free, higher fatigue strength) |
| Wear plate | Low impact with erosion-dominant duty | High chromium cast iron (GB/T 3226 series) or AR-grade low alloy wear steel — a hardness-controlled route that does not depend on work hardening |
10. Frequently asked questions
Why are two of the three components copper alloys and the third a cast steel?
The slide plate and the bushing both slide against a steel counterface under lubricated conditions, where a copper alloy gives a controlled wear rate and resistance to seizure. The wear plate serves a different function: it protects a structure against impact and abrasion, which calls for a hard chromium-bearing cast steel. Accepting the wear plate under a copper alloy standard would place it in the wrong material system, so it is listed and accepted separately.
What is the allowable limit for the bushing wall thickness?
Wall thickness should be at least 0.08 to 0.10 times the journal diameter. A 60 mm bore therefore requires a 5 to 6 mm wall. An alternative form used in practice is t = 0.05 × ID + (2 to 6) mm. The final value depends on load, length to diameter ratio and whether the component is centrifugal cast, since centrifugal castings are generally specified for bushings.
Why does the bushing need a larger running clearance than a tin bronze bushing?
Aluminium bronze has a coefficient of thermal expansion of approximately 17 × 10⁻⁶/K, above that of steel at approximately 11 × 10⁻⁶/K. As the assembly heats up, the bore closes faster than the shaft expands. A clearance of 0.1 to 0.2 % of shaft diameter compensates for this, and the value should be increased for high-temperature or high-speed duty. Insufficient clearance leads to binding and seizure.
Where should the oil groove be positioned on a bushing?
In the unloaded half of the bore. A groove located on the load line removes load-carrying area precisely where contact stress is highest, reducing capacity locally. Circumferential and axial grooves distribute lubricant, and separate debris grooves clear oxide scale particles that would otherwise act as a third-body abrasive.
Can the bushing grade run without a lubricant supply?
Not for sustained periods. ZCuAl10Fe3 contains no free-lead self-lubricating phase, so prolonged dry sliding leads to adhesive wear and rapid material transfer. Where oil cannot be supplied, the component should be changed to a solid-lubricant-embedded version of the same alloy base, or to a leaded grade suited to boundary lubrication.
Why does the hardness value on some material certificates appear as 980 HB?
That figure is a tensile strength in MPa, not a Brinell hardness. The specified hardness for this grade is 100 HBW minimum for sand casting and 110 HBW minimum for metal mould, continuous and centrifugal casting. An entry in that region should be corrected before acceptance, because hardness governs the wear relationship with the mating steel.
What is the difference between EN CC331G and CC333G?
CC331G is CuAl10Fe2-C, the iron-bearing aluminium bronze corresponding to C95400. CC333G is CuAl10Fe5Ni5-C, the nickel-bearing grade corresponding to the C95500 and C95800 group. They are different alloy systems with different corrosion behaviour and different heat-treatment response, so the designation must follow the standard named on the drawing.
What makes the wear plate grade suitable for impact duties only?
The grade achieves its wear resistance through work hardening. The surface must be subjected to impact or extrusion for the austenitic structure to transform and harden. Under low-stress sliding or continuous erosion the mechanism does not activate, and a hardness-controlled material such as high chromium cast iron will outlast it. This is why the duty description belongs on the purchase document.
Metal Bushing (Lubricated Metal) -Self-Lubricating Bushing Materials
Bushings are specialized, self-lubricating metal components widely utilized across various industries due to their durability and low maintenance requirements. Self-lubricating metal bushings are engineered to function without additional lubrication in numerous applications, thereby minimizing maintenance needs. These bushings are available in various series and configurations, such as flanged bushings and split bearings, to meet specific application requirements.
Metal-Polymer Anti-Friction Plain Bearings
Metal-Polymer Composite Self-lubricating Bushing Material
Steel Back + Porous Bronze Sinter + PTFE