Cone Crusher Bronze Bushings & Bearings: Material Selection for Mining and Aggregate Crushing
Maintenance-free Plain Bearings

Upload your file, choose your preferred production process and material, and get an instant quote.

Once your order is placed, production will begin, and you will receive regular status updates.

We guarantee quality assurance, supply detailed material reports, and offer delivery tracking.
Cone Crusher Bronze Bushings & Bearings: Material Selection for Mining and Aggregate Crushing
A structured reference for specifying bronze bearing components in cone crushers used across mining, quarrying and aggregate crushing plants — covering socket liners, eccentric bushings, countershaft bushings, thrust sets and the self-lubricating (graphite-plugged) option.
Cone-crusher bronze components are specified by matching the lubrication regime, contamination level, load magnitude and maintenance access of each position to the alloy’s tribological character. The two focus alloys are C93200 (SAE 660) for general duty and C93700 (SAE 64, “Grit Service”) for contaminated or boundary-lubricated duty. All limits shown are allowable (planning) values to be confirmed against the casting specification and mill test report.
VIIPLUS / Materials Coverage / Bearing Bronze / Cone Crusher Bronze Bushings
Graphite-Plugged Bronze Eccentric Bushings for Cone Crushers
Cone Crusher Bronze Sleeve & Bearing Material Selection
Application-position matrix and alloy-selection logic for socket liners, eccentric bushings, countershaft bushings and thrust sets — focused on C93200 (SAE 660) and C93700 (SAE 64, “Grit Service”) — in Mining & Quarrying and Aggregates & Crushing-Plant duty.
- C93200 General-duty, adequately-lubricated, medium-load/speed positions where machinability and cost efficiency dominate.
- C93700 Contaminated, gritty, or boundary-lubricated duty where higher lead/tin content improves anti-seizure, embeddability and dirt tolerance.
- Graphite-plugged Dusty, low-speed, maintenance-inaccessible pivot/oscillating positions — not a substitute for the oil film in sustained high-speed eccentric rotation.
Cone Crusher Bronze Bearing Positions & Duty
ronze is selected over steel for crusher journal surfaces because its softness and embedded lead phase embed abrasive particles and conform to minor misalignment, protecting the harder, more expensive shaft and frame. The positions below are ordered along the kinematic chain from drive to crushing head.
| Position | Function | Dominant duty | Lubrication regime |
|---|---|---|---|
| Eccentric bushing | Mounted in the eccentric assembly; converts countershaft rotation into the gyratory crushing stroke. Carries eccentric torque and high-speed sliding contact. | High radial load + sliding speed; shock/vibration | Oil-film (forced lubrication) |
| Countershaft / pinion-shaft bushing | Pressed into the countershaft box; supports the pinion shaft transmitting motor power at high RPM. | High rotational speed; heat buildup | Oil or grease |
| Socket liner / socket bushing | Seated in the socket; supports the spherical head (mantle assembly) underside against vertical crushing force and overturning moment. | Heavy axial + radial; overturning | Oil-film |
| Main-shaft / frame bushing | Fitted in the frame centre housing around the main shaft; primary radial bearing for the rotating head. | Massive radial crushing force | Oil-film |
| Head upper bushing | Guides the main shaft within the spider bore; precision fit governs mantle concentricity. | Precision guidance; light radial | Oil or grease |
| Spider bushing | Central pivot of the upper assembly; its failure is catastrophic to the machine. | Central pivot; shock-loaded | Oil or grease; often hard to access |
| Bottom-shell bushing | Supports the lower main-shaft end; maintains alignment within the bottom shell. | Alignment; low–medium speed | Oil or grease |
| Thrust bearing set | Multi-plate set (bronze plates with steel) managing axial thrust from crushing. | Axial thrust | Oil or grease |
| Piston wearing plate | Works with the socket liner to transmit hydraulic force and permit CSS adjustment. | Axial + sliding; hydraulic | Oil or grease |
eccentric bushings – Standard & Customized Bearings Alloy
Graphite-Plugged (Oilless) Bronze Bushings
Aluminium Bronze C95400 for Impact Zones
Manganese Bronze C86300 for Heavy Duty
Bearings for Mining & Aggregate Crushing
Heavy Duty Plain Bearings at viiplus.com. Solutions in Principal Markets Worldwide.
1. Why Bronze Is Specified for Cone Crusher Bearings
In a cone crusher, the bronze components act as the sacrificial, low-friction interface between rotating and stationary steel parts. Bronze is selected over steel for journal surfaces because its matrix and dispersed lead phase provide:
- Embeddability — small abrasive particles (rock dust, grit) embed into the softer bronze instead of scoring the harder steel shaft.
- Conformability — minor misalignment is absorbed, distributing load more evenly.
- Anti-seizure behaviour — the lead phase reduces the risk of galling if the lubricant film is lost briefly.
- Heat dissipation — the copper matrix conducts frictional heat away from the contact zone.
2. Cone Crusher Bronze Bearing Positions
The positions below are listed along the kinematic chain from the drive to the crushing head. Each carries a distinct duty that drives the alloy choice.
| Position | Function | Dominant duty | Lubrication |
|---|---|---|---|
| Eccentric bushing | Converts countershaft rotation into the gyratory crushing stroke; carries eccentric torque and high-speed sliding contact. | High radial load + sliding speed; shock | Forced oil film |
| Countershaft / pinion-shaft bushing | Supports the pinion shaft transmitting drive power at high RPM. | High rotational speed; heat | Oil or grease |
| Socket liner / socket bushing | Supports the spherical head underside against vertical crushing force and overturning moment. | Heavy axial + radial | Oil film |
| Main-shaft / frame bushing | Primary radial bearing for the rotating head inside the frame housing. | Massive radial crushing force | Oil film |
| Head upper bushing | Guides the main shaft in the spider bore; governs mantle concentricity. | Precision guidance | Oil or grease |
| Spider bushing | Central pivot of the upper assembly; failure is catastrophic to the machine. | Central pivot; shock | Oil or grease; often hard to access |
| Bottom-shell bushing | Supports the lower main-shaft end; maintains alignment. | Alignment; low–medium speed | Oil or grease |
| Thrust bearing set | Multi-plate set (bronze with steel) managing axial thrust from crushing. | Axial thrust | Oil or grease |
| Piston wearing plate | Works with the socket liner to transmit hydraulic force and allow CSS adjustment. | Axial + sliding; hydraulic | Oil or grease |
Focus Alloys: C93200 vs C93700
Both are continuous-, centrifugal- and sand-cast high-leaded tin bronzes. Minima below are continuous-cast values per ASTM B505/B505M unless noted; centrifugal and sand-cast specifications carry different minima for the same alloy — verify against the governing specification and the mill certificate (MTR).
C93200 — SAE 660 (Bearing Bronze, 83-7-7-3)
A general-duty bearing bronze for adequately-lubricated, medium-load and medium-speed positions. The lead phase provides short-interval lubrication if the film is lost.
Composition (ASTM B505/B584/B271, wt%)
| Cu | Sn | Pb | Zn | Ni≤ | Fe≤ | P≤ | Sb≤ |
|---|---|---|---|---|---|---|---|
| 81.0–85.0 | 6.3–7.5 | 6.0–8.0 | 1.0–4.0 | 1.0 | 0.20 | 0.15 | 0.35 |
EN equivalent ≈ CuSn7Zn4Pb7 (CC493K). Spec: SAE J461/J462; ASTM B505, B271, B584.
C93700 — SAE 64 (80-10-10, “Grit Service”)
Higher tin and lead than C93200. The elevated free-lead fraction gives improved anti-seizure, embeddability and conformability — it “envelops” foreign matter (rock dust, grit) and protects the mating steel surface.
Composition (ASTM B505/B505M, wt%)
| Cu | Sn | Pb | Zn≤ | Ni≤ | Fe≤† | Sb≤ | P≤‡ |
|---|---|---|---|---|---|---|---|
| 78.0–82.0 | 9.0–11.0 | 8.0–11.0 | 0.80 | 0.50 | 0.70 | 0.50 | ≤1.50 |
EN equivalent ≈ CuPb10Sn10 (CC480K, approximate). Spec: SAE J461/J462; ASTM B505, B271, B584, B22.
†Fe ≤0.35% when supplied as steel-backed. ‡ASTM B505/B505M-23 tabulates P up to 1.50%; several CDA-derived references list P ≤0.10–0.15 — confirm against the ordered specification.
Mechanical & physical comparison
| Property | C93200 (SAE 660) | C93700 (SAE 64) | Basis |
|---|---|---|---|
| Tensile strength, min | 241 MPa (35 ksi) | 241 MPa (35 ksi) | ASTM B505 |
| Yield strength (0.5% ext.), min | 138 MPa (20 ksi) | 138 MPa (20 ksi) | ASTM B505 |
| Elongation, min | 10% | 6% (typical 15–20%) | ASTM B505 |
| Brinell hardness (500 kgf), min | 65 HB | 60 HB | ASTM B505 |
| Density | 8.91 g/cm³ | 8.86 g/cm³ | 20 °C |
| Thermal conductivity | 58.2 W/m·K | 46.9 W/m·K | 20 °C |
| Machinability (C36000 = 100) | 70 | 80 | CDA |
| Solidus / Liquidus | 854 / 977 °C | 762 / 929 °C | — |
Hardness for leaded/tin bronzes is reported at a 500 kgf Brinell load; do not compare directly against aluminium/manganese bronzes reported at 3000 kgf.
4. Application-Position Matrix
Tags: Primary preferred for the stated duty · Suitable acceptable · Conditional only under the stated constraint · Not advised.
| Position | C93200 | C93700 | Graphite-plugged | Selection rationale |
|---|---|---|---|---|
| Eccentric bushing | Conditional | Primary | Not advised | Sustained high-speed rotation requires a forced oil film; C93700 tolerates grit ingress in mining feed. For the heaviest eccentric loads, escalate to higher-lead bronze (CuPb15Sn8 / C93800). Graphite cannot replace the hydrodynamic film here. |
| Countershaft / pinion-shaft bushing | Primary | Suitable | Not advised | High RPM demands heat dissipation — C93200’s higher thermal conductivity (58 W/m·K) and machinability suit this position; C93700 is an alternative where contamination is severe. |
| Socket liner / socket bushing | Suitable | Primary | Conditional | Heavy vertical + overturning loads favour the embeddable, anti-seizure character of C93700. Aluminium bronze (C95400) is considered where impact dominates. Graphite-plugged variants suit low-maintenance installations. |
| Main-shaft / frame bushing | Suitable | Primary | Not advised | Massive radial crushing force favours the conformable high-lead bronze; C93700 (or CuPb15Sn8 for heavier duty) reduces shaft scoring risk. |
| Head upper bushing | Primary | Suitable | Conditional | Precision guidance at moderate load; C93200 is adequate and economical, C93700 where grit is present. |
| Spider bushing | Conditional | Primary | Suitable | Catastrophic-failure position; premium leaded bronze (CuPb20Sn5 class) or C93700+ is standard. Graphite-plugged C95400 is an option where lubrication access is poor. |
| Bottom-shell bushing | Primary | Suitable | Not advised | Alignment-critical, lower-speed; C93200 is cost-effective, C93700 where contaminated. |
| Thrust bearing set | Primary | Suitable | Conditional | Axial plates (bronze/steel multi-plate); C93200/C93700 thrust plates are standard; graphite-plugged plates suit intermittent/low-speed axial duty. |
| Piston wearing plate | Primary | Suitable | Not advised | Works with the socket liner under hydraulic axial load; leaded tin bronze gives the needed embeddability. |
5. Material Selection Guide
Apply the decision chain in order; stop at the first binding constraint.
Both alloys are continuous-, centrifugal- and sand-cast high-leaded tin bronzes. Values below are continuous-cast minima per ASTM B505/B505M unless noted; centrifugal and sand-cast specifications carry different minima for the same alloy — verify against the governing specification and the mill certificate (MTR) for the casting route actually supplied.
C93200 — SAE 660 (Bearing Bronze, 83-7-7-3)
Workhorse general-purpose bearing bronze. Low friction, good machinability, adequate strength for medium duty. The lead phase provides short-interval “emergency” lubrication if the film is lost.
Composition (ASTM B505/B584/B271, wt%)
| Cu | Sn | Pb | Zn | Ni≤ | Fe≤ | P≤ | Sb≤ |
|---|---|---|---|---|---|---|---|
| 81.0–85.0 | 6.3–7.5 | 6.0–8.0 | 1.0–4.0 | 1.0 | 0.20 | 0.15 | 0.35 |
EN equivalent ≈ CuSn7Zn4Pb7 (CC493K). Spec: SAE J461/J462; ASTM B505, B271, B584.
C93700 — SAE 64 (80-10-10, “Grit Service”)
Higher tin and lead than C93200. The elevated free-lead fraction gives improved anti-seizure, embeddability and conformability — it “envelops” foreign matter (rock dust, grit) and protects the mating steel surface.
Composition (ASTM B505/B505M, wt%)
| Cu | Sn | Pb | Zn≤ | Ni≤ | Fe≤† | Sb≤ | P≤‡ |
|---|---|---|---|---|---|---|---|
| 78.0–82.0 | 9.0–11.0 | 8.0–11.0 | 0.80 | 0.50 | 0.70 | 0.50 | ≤1.50 |
EN equivalent ≈ CuPb10Sn10 (CC480K, approximate). Spec: SAE J461/J462; ASTM B505, B271, B584, B22.
†Fe ≤0.35% when supplied as steel-backed bearing. ‡ASTM B505/B505M-23 tabulates P up to 1.50%; several CDA-derived references list P ≤0.10–0.15 — confirm against the ordered specification.
Mechanical & physical properties
| Property | C93200 (SAE 660) | C93700 (SAE 64) | Test basis |
|---|---|---|---|
| Tensile strength, min | 241 MPa (35 ksi) | 241 MPa (35 ksi) | ASTM B505 |
| Yield strength (0.5% ext.), min | 138 MPa (20 ksi) | 138 MPa (20 ksi) | ASTM B505 |
| Elongation, min | 10% | 6% (typical 15–20%) | ASTM B505 |
| Brinell hardness (500 kgf), min | 65 HB | 60 HB | ASTM B505 |
| Density | 8.91 g/cm³ | 8.86 g/cm³ | 20 °C |
| Thermal conductivity | 58.2 W/m·K | 46.9 W/m·K | 20 °C |
| Machinability rating (C36000=100) | 70 | 80 | CDA |
| Solidus / Liquidus | 854 / 977 °C | 762 / 929 °C | — |
| Typical uses | General bushings, medium load/speed, thrust washers, pump & machine-tool bearings | High-speed/heavy-pressure bearings, dirty/gritty service, mine-water-exposed parts | — |
Hardness values for leaded/tin bronzes are conventionally reported at a 500 kgf Brinell load; do not compare directly against aluminium/manganese bronzes reported at 3000 kgf.
6. Allowable Operating Limits (Planning Reference)
The ceilings below are design reference / planning values for lubricated service, not guaranteed performance. Actual allowable limits depend on lubrication supply, surface finish (Ra), mating-shaft hardness, temperature and alignment. Verify against the supplier’s measured data and the MTR before specifying.
| Alloy | Allowable pressure (ceiling) | Allowable speed (ceiling) | Allowable PV (ceiling) | Binding constraint |
|---|---|---|---|---|
| C93200 (SAE 660) | ≈27.6 MPa (4 000 psi) | ≈3.8 m/s (750 fpm) | ≈2.6 MPa·m/s | PV usually binds before P |
| C93700 (SAE 64) | ≈27.6 MPa (4 000 psi) | ≈5.1 m/s (1 000 fpm) | ≈3.0 MPa·m/s | P binds first in eccentric positions |
| C93800 (CuPb15Sn8) | ≈17.2 MPa (2 500 psi) | ≈5.1 m/s (1 000 fpm) | ≈2.6 MPa·m/s | P binds early; higher speed at lower load |
Alternate planning basis (static / dynamic pressure, grease-lubricated, ambient): C93200 static ≈40, dynamic ≈20 N/mm², PV ≈3.5; C93700 static ≈35, dynamic ≈18 N/mm², PV ≈5.0. The two frameworks use different definitions — do not intermix. Derating is required above ~80 °C, with grease contaminated by rock dust or wash water, or with significant misalignment.
Graphite-plugged bronze (oilless) reference
| Property | Indicative value | Note |
|---|---|---|
| Static / dynamic allowable pressure | ≈60 / 25 N/mm² | Backing alloy dependent (C95400 / C86300 common) |
| Dry-running PV (planning) | ≈1.2 N/mm²·m/s | Lower than oil-lubricated solid bronze |
| Mating shaft hardness | ≥300 HB | Counterface Ra may relax to ≤1.6 µm |
| Graphite coverage | ≈10–30% area | Set by duty cycle and mating material |
7. Graphite-Plugged (Oilless) Bronze for Contaminated Duty
In mining, quarrying and aggregate plants, abrasive dust, intermittent heavy impact and limited maintenance access degrade conventional grease films. Graphite-plugged cast bronze removes the external-lubricant dependency: solid graphite transfers to the mating surface under load, forming a low-friction film (typical boundary μ ≈ 0.08–0.15).
- Preferred fit: low-speed / oscillating, dusty, hard-to-reach positions — crusher pivot arms, wear plates, spherical plain bearings, eccentric-shaft辅助 bearings where rotation is slow.
- Backing alloy: C95400 aluminium bronze or C86300 manganese bronze for load; C93200 base for lighter duty.
- Not a substitute: sustained high-speed eccentric rotation still requires a forced oil film — graphite cannot reach the hydrodynamic envelope of C93700 in that position.
8. Frequently Asked Questions
Which bronze is used for cone crusher eccentric bushings?
Eccentric bushings run under sustained high-speed rotation and require a forced oil film. C93700 (SAE 64, Grit Service) is preferred in contaminated mining feed because its higher lead and tin content improves anti-seizure and embeddability. For the heaviest eccentric loads, a higher-lead bronze such as CuPb15Sn8 / C93800 is considered. Graphite-plugged bronze is not a substitute in this position because it cannot reach the hydrodynamic envelope of the oil film.
What is the difference between C93200 and C93700 bronze?
Both are high-leaded tin bronzes. C93200 (SAE 660, roughly 83-7-7-3) is a general-duty bearing bronze for adequately-lubricated, medium-load and medium-speed positions, with higher thermal conductivity (about 58 W/m·K). C93700 (SAE 64, 80-10-10, Grit Service) carries more tin (9-11%) and lead (8-11%), giving improved anti-seizure, embeddability and conformability in gritty or boundary-lubricated service.
When should graphite-plugged bronze be used in a cone crusher?
Graphite-plugged (oilless) bronze suits low-speed or oscillating, dusty, hard-to-reach positions such as crusher pivot arms, wear plates and spherical plain bearings, where grease is routinely washed out. It is not intended for sustained high-speed eccentric rotation, which still requires a forced oil film.
Are the allowable load and speed values guaranteed performance?
No. Published allowable pressure, speed and PV figures are design reference or planning ceilings for lubricated service, not guaranteed performance. Actual limits depend on lubrication supply, surface finish, mating-shaft hardness, temperature and alignment, and must be verified against the supplier’s measured data and the mill test report.
Graphite / Oilless Option for Contaminated Duty
In Mining & Quarrying and Aggregates plants, abrasive dust, intermittent heavy impact and limited maintenance access degrade conventional grease films. Graphite-plugged cast bronze removes the external-lubricant dependency: solid graphite transfers to the mating surface under load, forming a low-friction film (typical boundary μ ≈ 0.08–0.15).
- Preferred fit: low-speed / oscillating, dusty, hard-to-reach positions — crusher pivot arms, wear plates, spherical plain bearings, eccentric-shaft bearings where rotation is slow.
- Backing alloy: C95400 aluminium bronze or C86300 manganese bronze for load; C93200 base for lighter duty.
- Not a substitute: sustained high-speed eccentric rotation still requires a forced oil film — graphite cannot reach the hydrodynamic envelope of C93700 in that position.