Crusher Bushing Alloy Selection
Crusher Bushing Alloy Selection
High-Performance Self-Lubricating Bronze Bushing Solutions & Technologies. Minimize downtime, extend service life, and reduce costs for dynamic applications.
Crusher Bushing Alloy Selection
Alloy data referenced to ASTM, SAE, EN and GB designations. Engineering guidance only — final selection must be confirmed against measured duty.
1 The governing principle
Selection principle
Bronze alloy selection in crushing equipment is decided by relative sliding speed — not by load. Load determines how much compressive strength you need. Sliding speed determines whether that strength is usable, or whether it becomes a liability.
Every crusher bushing position falls into one of two mechanical regimes, and the two require opposite material strategies.
| Regime | Dominant mechanism | Material family | Why |
|---|---|---|---|
| Low sliding speed, high compression |
Bore crushing, permanent deformation under load | Aluminium bronze C95400 / C95500 / C95800 Manganese bronze C86300 |
Almost no sliding means almost no frictional heat generation. Yield strength becomes the decisive property, and the poor embeddability of the harder alloys becomes irrelevant. |
| Rotating or rapidly oscillating |
PV heating, seizure, shaft scoring | Leaded tin bronze C93200 / C93700 / C93800 |
Lead supplies boundary lubrication when the oil film ruptures, and the soft matrix embeds abrasive particles instead of letting them cut the shaft journal. |
Warning
Consequence for specification
A hardness rule ofthumb used on all crusher positions will produce the wrong answer on at least one of them. Selecting by hardness alone is selecting incorrectly. Determine the sliding speed at the position first, then select the alloy family.
2 Position × alloy matrix
CSAQNACS = commonly specified | AQ = applicable with qualification | NA = not normally applicable| Position | Duty signature | C93700 C93800 |
C93200 | C90300 C90700 |
C95400 C95500 |
C95800 | C86300 | Solid lubricant |
|---|---|---|---|---|---|---|---|---|
| Eccentric bushing / eccentric sleeve |
Very high pressure, moderate to high speed, forced oil, shock from tramp material | ●︎ | ●︎ | ○︎ | ◐︎ | ◐︎ | ○︎ | ○︎ |
| Countershaft bush | Highest rotational speed in the machine, moderate pressure, forced oil | ◐︎ | ●︎ | ○︎ | ◐︎ | ○︎ | ○︎ | ○︎ |
| Socket liner / spherical bearing liner |
Very high axial load, slow gyration, hydrodynamic oil film, steel mating ball | ●︎ | ◐︎ | ○︎ | ○︎ | ○︎ | ○︎ | ◐︎ |
| Bottom shell bush / frame bushing |
High pressure, low speed, forced oil, carries full eccentric assembly | ◐︎ | ●︎ | ○︎ | ●︎ | ◐︎ | ●︎ | ○︎ |
| Spider bushing | Moderate pressure, oscillating, dusty, grease lubricated | ●︎ | ●︎ | ○︎ | ○︎ | ○︎ | ○︎ | ●︎ |
| Head bush, upper and lower |
Very high pressure, reversing, forced oil | ●︎ | ●︎ | ○︎ | ○︎ | ○︎ | ○︎ | ○︎ |
| Piston wearing plate / hydroset bushing |
Very high compression, very low speed, rotating against stationary piston | ◐︎ | ○︎ | ○︎ | ●︎ | ●︎ | ○︎ | ◐︎ |
| Thrust bearing / step plate |
Axial compression, very low speed | ◐︎ | ○︎ | ◐︎ | ●︎ | ●︎ | ◐︎ | ◐︎ |
| Jaw crusher eccentric shaft bush |
High cyclic pressure, moderate speed, shock load | ●︎ | ●︎ | ○︎ | ○︎ | ○︎ | ○︎ | ○︎ |
| Toggle seat / toggle plate bearing |
Very high pressure, oscillating, grease lubricated | ○︎ | ○︎ | ◐︎ | ●︎ | ◐︎ | ○︎ | ●︎ |
| Adjustment cylinder pin / pivot flange bush |
Static to intermittent, grease, dusty, frequent maintenance access | ●︎ | ●︎ | ○︎ | ●︎ | ○︎ | ○︎ | ●︎ |
| Curtain / apron pivot bush, breaker plate pin |
Static to intermittent, grease, dusty, high shock on tramp material | ●︎ | ●︎ | ○︎ | ●︎ | ○︎ | ○︎ | ●︎ |
2.1 How to read the matrix
Read across a row to see which alloy families suit a position; read down a column to see where one alloy family belongs. The pattern is not random. Radial positions on a rotating or precessing journal fall to the leaded bronzes, because embeddability and film-breakdown tolerance dominate. Compression-dominated positions with negligible sliding fall to the aluminium and manganese bronzes, because compressive capability dominates and there is very little sliding to generate heat.
Source basis: cncrusher.net large bronze bearing grade table; CSP Mühendislik spherical bearing and socket liner maintenance guide; Yile Machinery heavy industry plain bearing selection guide; Atlas Bronze shafting and journal material guidance.
3 Integrated selection recommendation
| Duty profile | Recommended grade | Selection logic |
|---|---|---|
| Slow-moving thrust or compression position, low frequency, oil supply reliable | ●︎ C95400 / C95500 | Compressive yield strength governs. The absence of significant sliding removes the main disadvantage of the harder alloys. |
| Rotating or oscillating journal, continuous forced oil, moderate load | ●︎ C93200 (SAE 660) | General-purpose bearing bronze. Good castability, good machinability, balanced wear resistance and thermal conductivity. |
| High-speed or rapidly oscillating, oil film intermittently broken, dusty environment | ●︎ C93700 / C93800 | Lead provides emergency boundary lubrication when the film ruptures, and embeds abrasive particles instead of transmitting them to the shaft. |
| Repetitive load cycles with abrasive wear, impact on tramp material | ●︎ C90700 / C90300 | Phosphorus refines grain structure and raises fatigue resistance under millions of load reversals. |
| Lubrication unreliable, intermittent service, inaccessible positions, high ambient temperature | ●︎ Aluminium bronze matrix with solid lubricant inserts | The matrix carries load; the embedded solid lubricant forms a transfer film. Note that solid lubricant occupies roughly 25–30 % of the bearing surface, so effective bearing area and load capacity must be recalculated accordingly. |
| Extreme structural load, low speed, older or specialised crusher designs | ●︎ C86300 manganese bronze | Highest strength of the cast bronze family. Selected where structural integrity under load outweighs machinability. |
| Seawater, brine, or continuous chloride exposure at a rotating position | ●︎ C95800 | The one regime where the nickel content earns its cost. Note that this is a marine duty condition — see section 5 before paying the premium. |
4 Shaft hardness: the requirement depends on alloy condition
Aluminium bronze contains no lead. It therefore has none of the anti-seizing reserve of a leaded bearing bronze, and substantially less conformability and embeddability. This makes the mating shaft a design variable rather than a detail. The requirement is stated in two tiers, and the correct tier depends on the hardness of the alloy itself.
| Aluminium bronze condition | Recommended mating shaft | Typical application |
|---|---|---|
| As cast, hardness about 140–170 HB | ≥ 400 HB min | C95800, C95500 and C95400 in as-cast condition. Most crusher main shaft journals, case or induction hardened, satisfy this. |
| Heat treated, hardness about 180–240 HB | > 500 HB, or HRC 60 min | Solution-treated and aged alloys, and manganese bronzes. Confirm the journal can achieve this before specifying a hardened condition. |
Warning
Do not substitute one bronze for another in isolation
Replacing a leaded tin bronze bushing with an aluminium bronze while leaving every other component unchanged is a frequent cause of early failure. The harder bushing transfers more wear to the mating surface. If the existing shaft journal is not hardened to the tier required by the selected alloy, the substitution accelerates damage to a component that is far more expensive than the bushing. Verify journal hardness, surface finish and lubrication supply before changing alloy family.
Source: Copper Development Association bearing guidance; Atlas Bronze shafting and journal material selection. For reference, crusher main shaft journals are commonly specified at HRC 50–56 in industry practice. Note that ASTM E140 hardness conversion tables are derived from non-austenitic steels and do not apply to copper alloys — a Brinell value for a bronze part should be read against the standard that specifies the test load.
5 Three specification traps that recur in crusher procurement
5.1 Listing multiple grades as equivalent alternatives
A requirement written as “BS 1400 AB2, ASTM C95800, JIS CAC703 or equivalent” is not a permissive specification. It is an unresolved conflict, because the composition ranges do not coincide.
| Element | BS 1400 AB2 | ASTM C95800 | JIS CAC703C | Common range | Issue |
|---|---|---|---|---|---|
| Al | 8.8–10.0 | 8.5–9.5 | 8.5–10.5 | 8.8–9.5 | Narrow |
| Fe | 4.0–5.5 | 3.5–4.5 | 3.0–6.0 | 4.0–4.5 | ≠︎ Narrowest — 0.5 wide |
| Ni | 4.0–5.5 | 4.0–5.0 | 3.0–6.0 | 4.0–5.0 | Workable |
| Mn | ≤ 3.0 | 0.8–1.5 | 0.1–1.5 | 0.8–1.5 | ≠︎ AB2 permits far more |
| Pb | ≤ 0.05 | ≤ 0.03 | ≤ 0.1 | ≤ 0.03 | Workable |
| Additional | — | Fe ≤ Ni | — | Fe ≤ Ni | ≠︎ Not required by AB2 |
Manganese is the decisive conflict: material certified as AB2-conforming may carry up to 3 % manganese and will be rejected under C95800, which caps the element at 1.5 %. The Fe ≤ Ni constraint in C95800 is a further rejection point that AB2 does not impose, so an AB2 certificate does not demonstrate C95800 conformance, and a C95800 certificate does not demonstrate AB2 conformance.
Mechanical minimums also differ, and the lower bound belongs to the UNS grade:
| Specification | Tensile (MPa) | 0.2 % proof (MPa) | Elongation (%) | Hardness (HB) | HB test load |
|---|---|---|---|---|---|
| BS 1400 AB2, continuously cast, min | 640 | 250 | 13 | — | not stated |
| EN 1982 CC333G, GC / GZ, min | 650 | 280 | 13 | ≥ 150 | not stated |
| ASTM B148 C95800, sand cast, min | 585 | 240 | 15 | ≥ 159 | 3000 kgf |
Recommendation
Recommended practice
Specify one governing standard, one casting method, one casting condition and one test-load basis for hardness. Where several designations must be permitted, attach the composition table above as an acceptance annex and state that the common range governs.
An intersection does exist and is commercially workable. For the grades above it is:
Cu ≥ 79.0 | Al 8.8–9.5 | Fe 4.0–4.5 | Ni 4.0–5.0 | Mn 0.8–1.5 | Pb ≤ 0.03 | Fe ≤ Ni
5.2 Brinell hardness without a stated test load
Lead content changes the appropriate Brinell test load for copper alloys. Leaded tin bronzes are normally evaluated at 500 kgf; aluminium and manganese bronzes at 3000 kgf. Two valid readings taken under different loads are not comparable, and a specification quoting a single hardness figure without the load cannot be verified. Always state the test load alongside the value.
5.3 Supplier grade tables that omit the alloying elements
Some published alloy tables list only the copper balance and residual impurity limits, without aluminium, iron, nickel or manganese. For an aluminium bronze these four elements are the alloy. A table that omits them imposes no technical requirement at all, and should not be used as a purchase basis. Verify against the ASTM, EN, BS or JIS document itself rather than a distributor page, and note that alloy tables for one grade sometimes differ between pages of the same source.
6 Paying for properties the duty does not require
C95800 nickel aluminium bronze is specified predominantly for seawater service. Its resistance to chloride corrosion, cavitation erosion and biofouling is the reason it carries a nickel premium. A crusher operating on aggregate, ore or quarried stone has no seawater duty, and in that environment the corrosion advantage is not exercised.
Where corrosion is not a specified requirement, C95400 aluminium bronze provides comparable compressive capability without the nickel content. Where the position is stationary relative to the shaft, the premium is entirely unnecessary. Comparing both grades against the same duty is a straightforward way to avoid paying twice for the same performance.
A second, opposite case is worth stating plainly. If the duty involves intermittent lubrication, abrasive dust, or a stated preference for the bushing to be sacrificed rather than the shaft journal, a high-leaded tin bronze is the correct answer and an aluminium bronze will score the journal. Aluminium bronze is harder and will therefore last longer in the wear test while causing more damage to the part it is protecting. Service life of the bushing alone is not the correct objective.
7 Geometry-based checks before quoting a drawing
Before a crusher bushing is treated as a standard catalogue item, four geometric checks resolve most ambiguities.
- Is the sliding speed physically possible? Peripheral speed follows from bore diameter and rpm. Large-diameter bushings leave the usable PV envelope for copper alloys at comparatively low rpm. If the computed PV exceeds the material limit by an order of magnitude, the duty description or the dimension is wrong — changing alloy will not resolve it.
- Is the spherical face present? A socket liner is a spherical plain bearing running against a hardened steel ball, with a hydrodynamic oil film. A plain cylindrical bore with no spherical radius cannot serve that function. Check for the spherical radius and for oil grooves or pockets, not just the bore diameter.
- Is there a register or flange? Positions carrying full axial load normally require a flange to locate the part and pins or a backing plate to retain it. A plain sleeve of uniform wall section indicates a different function.
- On split housings, how are the halves located? A split joint without a register or locating pins permits relative radial movement of the two halves at runtime. This fretting at the parting line is a recognised early failure mode for large split bronze bushings, and the locating feature should be defined on the drawing.
8 Alloy reference data
| Alloy | Designation | Density g/cm³ |
Tensile MPa |
Hardness HB |
Machinability % |
|---|---|---|---|---|---|
| Leaded tin bronze | C93700 / SAE 64 CuSn10Pb10 |
8.86–8.95 | 220–260 | 60–80 | 80 |
| High-lead tin bronze | C93800 CuSn7Pb13 |
9.25 | 205 min | 55–65 | 80 |
| Bearing bronze | C93200 / SAE 660 | 8.8–8.9 | 240 min | 60–70 | 70 |
| Phosphor bronze | C90700 | 8.8–8.9 | approx. 300 | 80–110 | 20–40 |
| Aluminium bronze | C95400 CuAl10Fe3 |
7.58 | 585 min | 170–210 | 60 |
| Nickel aluminium bronze | C95500 | 7.64 | 620 min | 190–230 | 50 |
| Nickel aluminium bronze | C95800 AB2 / CAC703 |
7.64 | 585 min | ≥ 159 | 50 |
| Manganese bronze | C86300 CuZn25Al6Fe3Mn3 |
8.3 | approx. 760 | approx. 225 | 20 |
Machinability referenced to free-cutting brass C36000 = 100 %. Hardness test load differs by alloy family — see section 5.2. Values are typical published figures for as-cast condition; the governing ASTM or EN document for the purchased grade always takes precedence. Permissible pressure and PV limits are not specified in SAE J461 or J462, which cover test method and acceptance criteria only — request a duty-specific verification from the supplier rather than relying on a catalogue figure.
9 Information required for a firm quotation
- Position of the part in the machine, and crusher make, model and size
- Rotational speed or sliding speed
- Radial and axial load
- Lubrication method and how reliable the supply is
- Mating shaft material, journal hardness and surface finish
- Working temperature and medium — dry, wet, slurry, or corrosive
- Supply condition — as cast, stress relieved, or heat treated
- Quantity per order and annual requirement
- Drawing with tolerances, fitting and any oil groove or drilling requirement
- Governing material standard and required certification level
Material certificates for copper alloy parts should reference the specific heat poured, state the casting method, and list measured chemistry rather than repeating a nominal alloy table. Test load, casting standard and heat number should each be stated on the document.
Metal Bushing (Lubricated Metal) -Self-Lubricating Bushing Materials
Bushings are specialized, self-lubricating metal components widely utilized across various industries due to their durability and low maintenance requirements. Self-lubricating metal bushings are engineered to function without additional lubrication in numerous applications, thereby minimizing maintenance needs. These bushings are available in various series and configurations, such as flanged bushings and split bearings, to meet specific application requirements.
Metal-Polymer Anti-Friction Plain Bearings
Metal-Polymer Composite Self-lubricating Bushing Material
Steel Back + Porous Bronze Sinter + PTFE