LG2 Bronze Bushings
LG2 Bronze Bushings
High-Performance Self-Lubricating Bronze Bushing Solutions & Technologies. Minimize downtime, extend service life, and reduce costs for dynamic applications.
LG2 Bronze Bushings: CC491K / C83600 Cast Copper Alloy Guide for Sliding Bearings
LG2 bronze bushings — also known as CC491K (BS EN 1982) and UNS C83600 (ASTM) — are leaded gunmetal castings with a nominal 85-5-5-5 composition (Cu-Sn-Pb-Zn). This guide covers verified chemical composition, mechanical minima by casting method, international equivalent grades, and allowable duty limits for screening bushing and sliding-bearing applications in this cast copper alloy.
Scope notice: This article covers one cast copper-tin-lead-zinc alloy (CC491K / C83600, legacy BS 1400 LG2) for general industrial bushings and sliding bearings. All values are provided as a data source for engineering evaluation only. This article contains no conclusion for military or defence use, automotive product approval, food contact, medical devices, nuclear applications, aviation airworthiness, or explosive atmospheres. Material property data presented here does not constitute an airworthiness finding, a certification basis, or any other certification conclusion.
Table of Contents
-
What Is LG2 Bronze?
-
Chemical Composition of CC491K / C83600
-
Equivalent Grades: LG2, CC491K, C83600, and More
-
Mechanical and Physical Properties
-
Why LG2 Bronze Is Used for Bushings
-
Allowable Duty Limits: PV, Pressure, Speed, Temperature
-
Where LG2 Bronze Fits — and Where It Does Not
-
Supply Forms, Certification, and Processing
-
Application Matrix for CC491K / C83600 Bushings
-
Selection Guide and Engineering Checklist
-
FAQ: LG2 Bronze Bushings
-
Appendix: Sources, Terminology, Units, Data Divergences
1. What Is LG2 Bronze?
LG2 is the grade designation used in BS 1400 (Specification for copper alloy ingots and copper alloy and high conductivity copper castings) for a leaded gunmetal: nominally 85% copper, 5% tin, 5% lead, and 5% zinc — commonly called 85-5-5-5. In North American usage, the same composition is known as ounce metal or leaded red brass.
BS 1400:1985 was superseded in 1999 by BS EN 1982, Copper and copper alloys — Ingots and castings (current edition BS EN 1982:2024). Drawings and purchase orders that still cite "BS 1400 LG2" map directly onto the current designation CC491K (CuSn5Zn5Pb5-C); the composition ranges are aligned. A dual designation on the order — LG2 (BS 1400) = CC491K (BS EN 1982) — closes out the withdrawn standard reference without changing the material.
LG2 is a casting alloy, not a wrought product. Supply forms include:
-
Sand castings
-
Gravity die castings
-
Centrifugal castings
-
Continuous cast bar or tube
Bushings are either cast near-net shape and machined, or turned from continuous cast bar (ASTM B505). The casting method matters: the tensile minimum is 200 MPa for sand castings and 250 MPa for centrifugal and continuous castings.
Table 1 — Function of Each Element in the 85-5-5-5 Composition (Nominal)
| Element | Nominal % | Function in the Alloy |
|---|---|---|
| Copper (Cu) | ~85 | Base matrix; corrosion resistance and thermal conductivity |
| Tin (Sn) | ~5 | Strength, hardness, and wear resistance of the bronze matrix |
| Zinc (Zn) | ~5 | Casting fluidity and deoxidation; lowers cost |
| Lead (Pb) | ~5 | Machinability (chip breaking), solid-lubricity, embeddability, and pressure tightness |
2. Chemical Composition of CC491K / C83600
The composition below is the requirement of BS EN 1982 for CC491K castings. Values are mass fractions in percent.
Table 2 — Chemical Composition of CC491K / C83600 / LG2, Castings
Basis: Standard, BS EN 1982 requirement
| Element | Min % | Max % | Note |
|---|---|---|---|
| Copper (Cu, incl. Ni) | 83.0 | 87.0 | Base |
| Tin (Sn) | 4.0 | 6.0 | Principal alloying element |
| Lead (Pb) | 4.0 | 6.0 | Principal alloying element |
| Zinc (Zn) | 4.0 | 6.0 | Principal alloying element |
| Nickel (Ni) | — | 2.0 | Residual |
| Iron (Fe) | — | 0.30 | Impurity |
| Antimony (Sb) | — | 0.25 | Impurity |
| Phosphorus (P) | — | 0.10 | Impurity; up to 1.5% permitted for continuous castings in ASTM B505 |
| Sulfur (S) | — | 0.10 | Impurity |
| Aluminium (Al) | — | 0.01 | Impurity; harmful to pressure tightness |
| Silicon (Si) | — | 0.01 | Impurity; harmful to pressure tightness |
3. Equivalent Grades: LG2, CC491K, C83600, and More
The grades below cover the same 85-5-5-5 composition family. Where a purchaser specifies "LG2 or equivalent," any of these designations denotes the same alloy; the choice is a documentation and market question, not a material change.
Table 3 — International Grade Equivalents for LG2 / CC491K / C83600
| System | Designation | Coverage |
|---|---|---|
| BS EN 1982 (current) | CC491K / CuSn5Zn5Pb5-C | Ingots and castings; suffix -GS sand, -GM metal mould (gravity die), -GZ centrifugal, -GC continuous |
| ASTM / UNS | C83600 | B62 (valve, flange, and fitting castings), B584 (sand castings), B271 (centrifugal), B505 (continuous cast bar/tube) |
| GB/T 1176 | ZCuSn5Pb5Zn5 | Chinese cast bronze designation (legacy ZQSn5-5-5) |
| JIS | BC6 | Japanese cast bronze, sand and metal mould |
| DIN EN 1982 | 2.1096.01 | Legacy DIN 1705 symbol G-CuSn5ZnPb (RG5) |
| ISO 1338 | CuPb5Sn5Zn5 | Cast copper alloy designation |
| NF (France) | CuPb5Sn5Zn5 | Cast copper alloy designation |
| AS 1565 (Australia) | C83600 / 836B | Cast bronze |
| Legacy cross-reference only | SAE 40; QQ-C-390; MIL-C-15345 Alloy 1 | Historical drawing-conversion references; SAE 40 discontinued. These carry no military, defence, or airworthiness qualification meaning. |
4. Mechanical and Physical Properties
Mechanical minima differ by casting method because density and cooling rate differ. Always confirm which method applies to the supplied form.
Table 4 — Mechanical Minima for CC491K
Basis: Standard, BS EN 1982 requirement
| Casting Method (Suffix) | Tensile Rm, MPa ≥ | 0.2% Proof Rp0.2, MPa ≥ | Elongation A, % ≥ | Hardness HBW ≥ |
|---|---|---|---|---|
| Sand casting (GS) | 200 | 90 | 13 | 60 |
| Metal mould / gravity die (GM) | 220 | 110 | 6 | 65 |
| Centrifugal casting (GZ) | 250 | 110 | 13 | 65 |
| Continuous casting (GC) | 250 | 110 | 13 | 65 |
Table 5 — ASTM Cross-Check for C83600
Basis: Standard, ASTM requirement
| Specification | Tensile, MPa ≥ | Yield, MPa ≥ | Elongation, % ≥ |
|---|---|---|---|
| B584 / B62, sand casting | 207 (30 ksi) | 97 (14 ksi) | 20 |
| B505, continuous casting | 248 (36 ksi) | 131 (19 ksi) | 15 |
Table 6 — Physical and Typical Properties
Basis: Typical, manufacturer-published indicative values, not minimums
| Property | Value | Note |
|---|---|---|
| Hardness | 60–75 HB | Soft matrix; tolerant of unhardened shafts |
| Machinability | 84–90% of free-cutting brass | Lead phase breaks chips |
| Density | ≈8.8 g/cm³ | — |
| Modulus of elasticity | ≈93–105 GPa | — |
| Melting range | 854–1010 °C | — |
| Thermal conductivity | ≈71 W/(m·K) | Moderate; dissipates friction heat at low speeds |
| Coefficient of thermal expansion | ≈18 × 10⁻⁶ /K | — |
| Maximum working temperature | 225–230 °C | Long-term service ceiling |
5. Why LG2 Bronze Is Used for Bushings
LG2 / CC491K / C83600 offers a combination of properties that make it a reliable choice for general-purpose sliding bearings:
-
Embeddability and conformability. The free lead phase lets the bushing absorb grit and conform to shaft deflection, protecting the shaft during boundary lubrication and brief oil interruption.
-
Anti-seizure margin. Lead provides a solid-lubricity film at the surface, so the alloy tolerates marginal lubrication better than unleaded tin bronzes of similar cost.
-
Machinability. At 84–90% of free-cutting brass, bores, oil grooves, and close tolerances are economical to machine.
-
Corrosion behaviour. Published foundry data describe good resistance in freshwater and atmospheric exposure, resistance to dezincification, and reasonable behaviour in seawater and brine — but not for acidic or abrasive media.
-
Non-sparking character. Like other copper alloys without beryllium, it is commonly selected for environments where impact sparking must be avoided (typical basis).
-
Pressure tightness. Relevant when the same alloy is used for cast valve bodies and pump casings: lead fills micro-shrinkage and gives leak-tight castings.
6. Allowable Duty Limits: PV, Pressure, Speed, Temperature
For continuous sliding, the controlling parameter is the pressure-velocity product (PV), not a peak static load. Screen the application with:
p = W / (d · L) (MPa, with W in N and d, L in mm)
v = π · d · n / 60000 (m/s, with d in mm and n in rpm)
Require: p · v ≤ PV limit
Worked example: A bushing with d = 50 mm, L = 50 mm carrying W = 10 kN at n = 100 rpm gives p = 4.0 MPa and v = 0.26 m/s, so p·v = 1.05 MPa·m/s — inside the lubricated limit below.
Table 7 — Duty Limits for CC491K / C83600 Bushings
Basis: Typical, supplier-published indicative values; not standard minimums
| Parameter | Allowable Limit | Note |
|---|---|---|
| PV, lubricated (oil or grease) | ≈1.65–1.75 MPa·m/s | Two independent supplier datasets converge (≈50,000 psi·ft/min) |
| PV, dry friction | ≈1.0 MPa·m/s | Lead film only; not for continuous dry running |
| Sliding speed, lubricated | ≤2.5 m/s | Low-to-medium speed duty |
| Sliding speed, dry | ≤0.5 m/s | Oscillating or intermittent duty |
| Maximum working temperature | 225–230 °C | — |
| Peak / static pressure | Published values diverge: 8 MPa (screening value) vs 50 MPa (supplier sample) | Screen at the lower bound; do not average. See Appendix, data divergences. |
7. Where LG2 Bronze Fits — and Where It Does Not
Compared with other bronze grades commonly offered for bushings, CC491K / C83600 occupies the general-purpose, machinable, moderate-duty slot.
Table 8 — Material Comparison for Bushing Screening
Basis: Typical, engineering-reference values from supplier and handbook data; screen at the lower bound
| Material | Lubricated PV Limit, MPa·m/s | Indicative Pressure Capability, MPa | Character | Screen Use When |
|---|---|---|---|---|
| CC491K / C83600 (this grade) | ≈1.65–1.75 | 8 (screening) – 50 (sample, see divergence note) | Machinable, embeddable, pressure-tight castings | Moderate load, lubricated, low-to-medium speed |
| Oil-impregnated sintered bronze (SAE 841, ASTM B438) | ≈1.6–1.8 | 14–15 | Oil stored in pores; low speed | Light duty, inaccessible lubrication points |
| C93200 / SAE 660 (83-7-7-3) | ≈2.6–3.0 | ≈27.6 | Higher-duty general bearing bronze | Higher load or speed than this grade |
| Aluminum bronze C95400 (CuAl10Fe3) | ≈4.4 | ≈41.4 | High strength, hard, wear-resistant | Heavy load, marine or abrasive media |
| Aluminum bronze C95500 (CuAl9Fe4Ni4Mn2) | Higher than C95400 | Higher than C95400 | Heavy marine and shock duty | Propeller-adjacent and shock-loaded positions |
| Graphite-plugged cast bronze | ≈1.0 (dry) | — | Solid lubricant in the wall | No lubrication access, dry or intermittently dry duty |
8. Supply Forms, Certification, and Processing
8.1 Casting Method and Purchase-Order Wording
State the casting method on the purchase order: the tensile minimum moves from 200 MPa (sand) to 250 MPa (centrifugal or continuous). For turned bushings, continuous cast bar per ASTM B505 is the common route and carries the higher minima.
8.2 Material Inspection Documents (EN 10204)
Table 9 — EN 10204 Document Types
Basis: Standard, EN 10204 content definitions
| Type | Content |
|---|---|
| 2.1 | Declaration of conformity, no test results |
| 2.2 | Non-specific test report |
| 3.1 | Specific inspection of the supplied lot: test results traceable to the heat |
| 3.2 | As 3.1, plus the purchaser's or an official inspector's witness |
These are supplier quality documents. None is a sector approval and none is an airworthiness release.
8.3 Processing Notes
-
Welding: Generally not recommended for this leaded grade because of lead fume and cracking risk. One foundry publishes successful TIG/MIG repair guidance with matching filler; treat that as unverified and qualify by procedure test. Brazing and soldering are feasible.
-
Stress relief: Approximately 260 °C, 1 h per 25 mm of thickness (typical).
-
Machining: Standard practice; lead acts as a chip breaker. Fine bores and oil grooves are routine.
8.4 Lead Content and Market Restrictions
The grade carries 4–6% lead. The RoHS Annex III exemption 6(c) for copper alloys is limited to 4% lead by weight, so this composition sits above that ceiling; lead-restricted applications call for lead-free grades such as tin bronze or aluminum bronze, and the current consolidated directive text should be checked for the end market. Lead-bearing alloys may also trigger REACH Candidate List communication duties depending on form and current list status. For potable-water and food-contact positions, separate lead-limit regimes apply and are not evaluated in this article.
8.5 Sector Certification Boundary
Table 10 — What This Document Does Not Provide, by Sector
| Sector | Applicable Regime | What This Document Does Not Provide |
|---|---|---|
| Aerospace | EASA/FAA Part 21, AS9100, NADCAP | No airworthiness finding or certification basis |
| Defence | ITAR 22 CFR 120-130, EAR 15 CFR 730-774 | No export-control or qualification conclusion |
| Automotive | IATF 16949 (organisation-level) | No product approval conclusion |
| Food contact | EC 1935/2004, EU 10/2011, 21 CFR 177.1550 (resins) | No food-contact suitability conclusion |
| Medical devices | EU MDR 2017/745, FDA device regulation | No device classification or approval conclusion |
| Nuclear | ASME NQA-1, RCC-M | No nuclear qualification conclusion |
| Explosive atmospheres | ATEX 2014/34/EU, EN ISO 80079-36/-37 | No category, EPL, or temperature class assigned |
9. Application Matrix for CC491K / C83600 Bushings
Table 11 — Typical Positions for CC491K / C83600 Bushings
| Equipment / Assembly | Position | Motion and Load | Environment | Suitability |
|---|---|---|---|---|
| Rotodynamic pumps | Shaft sleeves, impeller wear rings, gland bushings | Continuous rotation, low-to-medium load | Fresh water, oils | Within PV limit |
| Valves (water, low-pressure steam) | Stem guides, seat bushings | Intermittent stroke, low load | Water, steam up to ≈225 °C | Within limits; casting pressure tightness also relevant |
| Marine deck hardware | Rudder stock bushings, winch pivots | Oscillating, light-to-medium load | Seawater splash | Usable; heavy or continuous marine duty → aluminum bronze |
| Conveyor systems | Roller end bushings, idler pivots | Continuous slow rotation | Dust, occasional grit | Embeddability helps; abrasive mineral duty → re-evaluate |
| Agricultural machinery | Linkage pivots, harvester joints | Oscillating, shock | Dirt, washdown | Usable where lubrication access exists |
| Hydraulic cylinders | Gland bushings, clevis bushings | Reciprocating | Hydraulic oil | Light-to-medium duty |
| General engineering | Light-duty gears, worm wheels | Low speed | General | Only where loading is small |
10. Selection Guide and Engineering Checklist
Table 12 — Quick Selection Guide
| If the Duty Is… | First Choice | Reason |
|---|---|---|
| Moderate load, lubricated, low-to-medium speed | CC491K / C83600, cast or continuous cast | Machinable, embeddable, within PV limit |
| Higher load or speed | C93200 (SAE 660) | Higher PV and pressure capability |
| Heavy load, marine, or abrasive media | Aluminum bronze C95400 / C95500 | Higher strength, PV, and abrasion tolerance |
| No lubrication access | Graphite-plugged cast bronze, or oil-impregnated sintered bronze (ASTM B438) | Solid or stored lubrication |
| Lead-restricted market | Lead-free tin bronze or aluminum bronze | Pb content of this grade exceeds the RoHS 6(c) ceiling |
Essential Checklist — Confirm Before Quoting
-
Bore, outside diameter, length, and tolerance class — from drawing or measured sample
-
Casting method (GS / GM / GZ / GC) — tensile minimum differs by method (200 vs 250 MPa)
-
Lubrication regime and relubrication access — dry positions need a different design route
-
Calculated p and v, and p·v against the PV limit — Table 7
-
Shaft hardness and surface finish — the soft matrix tolerates unhardened shafts, but check the pairing
-
Environment — abrasive media, acidic water, or stagnant seawater change the choice
-
Lead restrictions for the end market — potable water, food contact, RoHS-scope products
-
Purchase-order designation — dual "LG2 (BS 1400) = CC491K (BS EN 1982)" closes the withdrawn standard
11. FAQ: LG2 Bronze Bushings
What is LG2 bronze?
LG2 is the BS 1400 designation for a leaded gunmetal casting bronze with a nominal 85-5-5-5 composition (85% Cu, 5% Sn, 5% Pb, 5% Zn), also known as ounce metal or leaded red brass. BS 1400 was superseded in 1999 by BS EN 1982; the current designation for the same alloy is CC491K (CuSn5Zn5Pb5-C), and UNS C83600 in the ASTM system.
Is BS 1400 LG2 the same as C83600?
Yes. C83600 covers the same 85-5-5-5 composition family under ASTM B62 (valves and fittings), B584 (sand castings), B271 (centrifugal castings), and B505 (continuous castings). Where a drawing states LG2 or equivalent, any of CC491K, C83600, ZCuSn5Pb5Zn5, or JIS BC6 denotes the same alloy.
What do the EN 1982 suffixes GS, GM, GZ, and GC mean?
They identify the casting method: GS sand casting, GM metal mould (gravity die) casting, GZ centrifugal casting, GC continuous casting. The mechanical minima differ by method, with a tensile minimum of 200 MPa for sand castings and 250 MPa for centrifugal and continuous castings.
What is the allowable PV for an LG2 / C83600 bushing?
Published indicative values place the lubricated PV limit at roughly 1.65 to 1.75 MPa·m/s and the dry-friction limit near 1.0 MPa·m/s, with sliding speeds up to about 2.5 m/s lubricated and 0.5 m/s dry. These are typical supplier values rather than standard minimums; screen the design with p = W/(d·L) and v = π·d·n/60000.
Can LG2 / C83600 bushings run without lubrication?
The lead phase provides anti-seizure margin under boundary lubrication and brief oil interruption, but continuous dry running exceeds the dry PV limit of about 1.0 MPa·m/s. For positions without lubrication access, self-lubricating designs such as graphite-plugged cast bronze or oil-impregnated sintered bronze (ASTM B438) are the usual route.
12. Appendix: Sources, Terminology, Units, Data Divergences
A.1 Sources Consulted (October 2026)
-
BS EN 1982 (Copper and copper alloys — Ingots and castings), composition and mechanical minima for CC491K / CuSn5Zn5Pb5-C, cross-checked against published DIN EN 1982 composition data.
-
ASTM B62 / B584 / B505 / B271 for C83600 composition and mechanical requirements, cross-checked against foundry data sheets.
-
BSI / NSAI standards records for the status of BS 1400:1985 (superseded 1999 by BS EN 1982; current edition BS EN 1982:2024).
-
Published mill and foundry data sheets for LG2 / CC491K and C83600 (typical properties, bearing duty statements, processing notes).
-
GB/T 1176 and JIS BC6 designation and composition references.
A.2 Terminology Conventions
-
Standard vs Typical. "Standard" values are requirements of the cited document (minima). "Typical" values are manufacturer-published indicative figures, not minimum values. The two are labelled separately in every table and never merged.
-
Allowable limit. "Allowable limit" denotes a screening ceiling for engineering use; "maximum" is used only as an engineering parameter (maximum working temperature, maximum sliding speed, maximum PV).
-
Casting suffixes. GS sand, GM metal mould (gravity die), GZ centrifugal, GC continuous, per BS EN 1982.
A.3 Unit Conversions
-
1 psi = 6.895 kPa; 1 ksi = 6.895 MPa
-
1 psi·ft/min = 3.503 × 10⁻⁵ MPa·m/s (so 50,000 psi·ft/min ≈ 1.75 MPa·m/s)
-
Sliding speed: v = π·d·n/60000 m/s with d in mm and n in rpm
-
Projected bearing area: d × L in mm²; p = W/(d·L) in MPa with W in N
A.4 Known Data Divergences Between Sources
-
Peak / static pressure: Published values for this grade range from an 8 MPa recommended screening value to a 50 MPa supplier sample figure. Both are published here; screen at the lower bound. Do not average.
-
Typical tensile strength: One foundry quotes 240–280 MPa typical for castings; the standard minima are 200 MPa (sand) and 250 MPa (centrifugal / continuous). Typical values are indicative and sit above minima by definition.
-
Welding: Most data sheets state welding is not recommended for this leaded grade; one foundry publishes TIG/MIG repair guidance. Treated as unverified in this article.
-
Maximum working temperature: 225 °C and 230 °C both appear in published data; the range 225–230 °C is used here.
-
Lubricated PV: Supplier datasets converge at 1.65–1.75 MPa·m/s; the range is published rather than a single point.
Keywords: LG2 bronze bushings, CC491K, C83600, leaded gunmetal, 85-5-5-5 bronze, cast copper alloy, sliding bearings, bronze bushing material, BS EN 1982, ASTM B505, PV limit, bearing duty limits, leaded red brass, ounce metal, CuSn5Zn5Pb5-C.
Metal Bushing (Lubricated Metal) -Self-Lubricating Bushing Materials
Bushings are specialized, self-lubricating metal components widely utilized across various industries due to their durability and low maintenance requirements. Self-lubricating metal bushings are engineered to function without additional lubrication in numerous applications, thereby minimizing maintenance needs. These bushings are available in various series and configurations, such as flanged bushings and split bearings, to meet specific application requirements.
Metal-Polymer Anti-Friction Plain Bearings
Metal-Polymer Composite Self-lubricating Bushing Material
Steel Back + Porous Bronze Sinter + PTFE