Trolley Reeving System Bushing: Application Matrix and Bronze Material Selection

Trolley Reeving System Bushing: Application Matrix and Bronze Material Selection

High-Performance Self-Lubricating Bronze Bushing Solutions & Technologies. Minimize downtime, extend service life, and reduce costs for dynamic applications.

Custom Bronze Bearings for Sugar Mill (LBC-3) GRAPHITE SELF-LUBRICATING BEARING

Trolley Reeving System Bushing: Application Matrix and Bronze Material Selection

A trolley reeving system bushing sits between the sheave hub and its pin, carrying rope traction as a radial load through repeated start-stop cycles. This guide maps the duty to candidate sites, then maps each site to a bronze grade, a graphite plug pattern and a verifiable pressure limit.

Engineering reference · Plain bearing selection · Bronze and copper-base alloys · Values are design reference ceilings, not guaranteed performance

Scope. This document covers solid-lubricated (graphite-plugged) bushings for crane trolley and reeving service. It covers application position, duty characterisation, grade selection, plug layout, and the checks required before a grade can be released for production. Wrapped bimetal bushings, rolling-element bearings and polymer bearings are outside scope except where they appear as alternatives.

01What the component does

The bushing is a plain bearing pressed or fitted into the sheave hub, with the sheave pin passing through its bore. Its job is to convert the radial component of rope tension into a distributed pressure over the bore surface, while limiting friction so that the pin does not seize and the hub does not wear.

Three features of this duty shape every material decision:

  • Radial load from rope traction. The load follows the rope line and rotates with the sheave as the boom or trolley travels.
  • Intermittent rotation. Trolley sheaves accelerate, hold, brake and reverse repeatedly. Duty is characterised by starts per hour rather than continuous speed.
  • Restricted lubrication access. The bushing sits inside the hub. Disassembly requires pressing out the sheave, so scheduled regreasing is impractical. This is the reason a self-lubricating construction is specified.

02Why a self-lubricating construction is used

In a graphite-plugged bushing, solid lubricant plugs are press-fitted into machined cavities across the sliding surface. Under load and motion, lubricant transfers from the plug surface onto the pin, building a transfer film that separates metal from metal. The plugs are consumed slowly; the metal substrate carries the structural load rather than wearing away.

Two consequences follow, and both matter when reading a drawing:

  • The base alloy and the lubricant are selected together. A base alloy chosen for strength but unable to retain plugs gives a bushing that either seizes or wears its bore.
  • The mechanism depends on plugs being present in the loaded zone. Plug layout is a design variable with rules, not a decorative feature. Coverage is commonly 20 to 30 per cent of the sliding surface.

Plug layout rules

Table 1 — Constraints that govern a plug pattern
Rule Reason
Plugs must not cross an oil groove A groove crossing a plug interrupts film continuity and leaves an unwetted band at the groove root.
Plugs must not cross a split line The split is a discontinuity in the substrate; plugs spanning it lose retention as the halves move.
Coverage held near 20 to 30 per cent Below that range film continuity is unreliable; above it the substrate loses load-carrying section and plug retention falls.
Coverage continuous through the full arc of oscillation For an oscillating pivot the swept arc is narrower than the full circumference, so plugs outside that arc contribute nothing.
Staggered rather than concentric rows Concentric rings line up into continuous radial grooves under wear, weakening circumferential section. Staggering spreads contact across the surface.

03Application position matrix

The table below lists the positions where a trolley-type bushing is found in crane and hoist service, with the duty each position imposes. Positions are grouped by the constraint that actually governs material choice, because the governing constraint — not the position name — is what decides the grade.

Table 2 — Trolley and reeving application position matrix
Position Load path Duty Lubrication access Candidate material Governing constraint
Trolley rope sheave pin
Trolley running sheave, rope deflection sheave
Radial, rope tension Intermittent, reversing Restricted C95400 or C86300 with graphite plugs Start-stop shock combined with rope load fluctuation; pin alignment varies as the rope moves across the sheave.
Hook block sheave pin Radial, variable Intermittent, shock Restricted C86300 with graphite plugs Shock load from hoisting and snagging. Ranks in the upper load class among sheave positions; housing bore is not a wear surface here.
Boom head and jib tip sheave pin Radial, rope tension Continuous, low speed Restricted C95400 or C95500 with graphite plugs Sustained rope load with low rotation. Corrosion exposure from weather; aluminium bronze oxide film assists here.
Counterweight sheave pin Radial, tension Continuous, low speed Restricted C95400 with graphite plugs High static load, little rotation. Plug retention under sustained load governs; creep of the substrate matters more than wear.
Luffing and slew joint pivot Radial plus axial thrust Slow oscillation Poor C86300 with graphite plugs Thrust plus oscillation in one component. Frequently requires a flanged form to carry axial load rather than a plain sleeve.
Rope guide and anti-two-block device Guide contact Oscillating Poor C95400 with graphite plugs Sawtooth motion through a limited arc. Plug coverage must lie inside that arc, not around the full circumference.
Sheave keeper plate and retainer pin Retaining Static Not applicable Stainless or plated steel Not a sliding duty. A sliding bushing is the wrong component here; retention and corrosion resistance govern.
Trolley travel wheel Rolling contact Rolling Accessible Rolling-element bearing A trolley wheel runs on a rail and rolls. A plain bushing is not applicable; the wheel uses a rolling bearing and a tyre.
Drum end bearing and rope retainer Thrust Static to slow Restricted C93200 or C95400, oil-lubricated Thrust duty, limited sliding distance. Access permits grease, so a lubricated bronze is usually more economical than a plugged grade.

Read across, not down. A single part number may appear in several of these positions, but the acceptable grade changes with duty. The same trolley sheave pin drawing can be acceptable in one position and rejected in another, because the shock content and the lubrication access differ. Confirm the position before confirming the grade.

04Material selection

Table 3 lists the copper-base grades normally considered for these positions. Values are taken from published standards and supplier data as design reference ceilings for the duty named. They are not guaranteed values and they assume the lubrication condition stated.

Table 3 — Candidate grades for trolley and reeving plain bearings
Grade Tensile
MPa typ.
Hardness
HB typ.
Allowable pressure ceiling
MPa
Allowable PV ceiling
MPa·m/s
Notes on use in this duty
SAE 841
CuSn10Fe, sintered
~300 (crush) 45–65 14–15 1.6–1.8 Below the load class of a rope sheave. Oil impregnation supplies lubrication, but the porous structure is vulnerable to abrasive dust and cannot be machined after sintering without closing the pores. Listed here for completeness of comparison.
C93200 / C93700
Leaded tin bronze
241 60–65 27.6 2.6–3.0 Embeddable and conformable, which suits debris. Lead content restricts use where food contact or plating rules apply. Below the load class of a main rope sheave.
C90700
Lead-free tin bronze
262–310 80 34.5 3.5 Lead-free option with a higher speed ceiling than the leaded grades. Still below the load class of a main rope sheave.
CuSn12
CC483K, phosphor bronze
250–400 100–150 60 — Hard delta phases give good anti-seizure behaviour. Requires adequate lubrication; strength depends heavily on casting method. Relevant where a lubricated pin joint replaces a plugged bushing.
C95400
CuAl10Fe3, aluminium bronze
517–586 150–170 41.4 4.4 Iron-rich phase gives good wear resistance; oxide film handles weather exposure. A standard base alloy for graphite-plugged bearings. Cost-effective where corrosion is secondary.
C95500
CuAl9Fe4Ni4Mn2, NAB
620–655 190–230 High High Nickel content raises strength and fatigue resistance. Used where shock and load combine, and where water contact is persistent. Brinell rises to roughly 208 in the referenced specification.
C95800
CuAl10Ni5Fe4, NAB
585 150–190 High High Lowest aluminium content of the nickel aluminium bronze family; greater resistance to dealuminification in continuous immersion than the other members of the family. Relevant to marine service rather than to dry crane service.
C86300
CuZn25Al6Fe3Mn3, manganese bronze
758–827 225 Very high static — Greater strength than the other grades in this group, with high impact toughness. The reference grade for high-load graphite-plugged bushings. This is the grade that matches a drawing calling for hardness in the 210 to 240 HB range with tensile above 700 MPa.
Graphite-plugged build
C95400 / C95500 / C86300 base, 20–30 per cent graphite
Base value Base value 100–120 static
~70–90 dynamic
~1.65 dry Published figures for plugged builds differ by source and by base alloy; one source places dynamic capability near 70 MPa for a C95400 base and 100 to 120 MPa for the nickel aluminium bronze family. Dry sliding speed is typically held at or below 0.5 m/s. Treat these as ceilings requiring confirmation against supplier data.

Reading the pressure column. The allowable pressure ceiling and the PV ceiling are different constraints, and the smaller one governs. A grade with a high pressure ceiling can still be limited by PV as soon as the pin rotates at speed. Both figures must be checked against the actual duty; neither alone is sufficient.

Selection by governing constraint

Table 4 — Constraint-led grade selection
Governing condition Grade to consider first Reason
Moderate load, oil access available C93200 or C93700 Embeddability and conformability; lower cost. Regreasing is possible, so a plugged grade is not required.
Heavy load, low speed, no lubrication access C86300 with graphite plugs Strength carries the static load; plugs supply the film. This combination addresses the trolley sheave pin duty directly.
Load plus weather or water exposure C95400 or C95500 with graphite plugs Aluminium bronze oxide film tolerates exposure better than tin bronze, and resists abrasion in a dirty environment.
Severe shock with large section C86300 with graphite plugs Impact toughness and static strength; low creep under sustained load.
Lead-free or plating-rule compliance C95400 or CuSn8Ni Aluminium bronze is naturally lead-free; avoids leaded tin bronze where contact rules apply.
Continuous immersion in seawater C95800 Dealuminification resistance; outside the dry crane duty but relevant to port and marine cranes.

05Plug pattern design

Plug layout decides whether the self-lubricating mechanism works. Two patterns produce similar plug counts but behave differently in service.

A · Concentric ringsPlugs in line across the diameter.Wear joins rings into a continuous radial groove,reducing circumferential substrate section.B · Staggered rowsRows offset by half pitch; no continuous radial line.Contact spreads across the surface and thesubstrate retains section between plug rows.
Figure 1 — Ring alignment against staggered rows. The plug count is similar in both patterns; the difference is how the pattern degrades as wear proceeds.

06Worked reference: a trolley sheave bushing

Reference drawing J580A210311, titled trolley reeving system bushing, is used here as the worked example. Dimensions below were verified against the drawing geometry.

Table 5 — Reference bushing, verified dimensions
Feature Dimension Note
Bore, working surface ∅100 H9 (+0.087 / 0) Hole basis. Clearance fit on the pin.
Body outside diameter ∅120 s6 (+0.101 / +0.079) Shaft basis. Fit into the hub.
Flange diameter ∅136 One end only; thrust and location feature.
Overall length 57 Effective bore length approximately 55.
Flange thickness 14 —
Annular groove 8 wide, centre 33 from face Reservoir for grease or film.
Bore relief ∅105 Both ends. Tool run-out and clearance.
Plug pattern 16 shown, 4 rows staggered Rows at nominal radii 9.4, 21.1, 31.6 and 42.1 from the axis. Pattern follows the staggered rule in Table 1.
Chamfer 1 × 45° Both ends.
Surface roughness Ra 3.2 Sliding surfaces.
Perpendicularity 0.025 to A Datum A.
Unspecified linear tolerance 12.5 Micrometre class.

Reading the material call-up against the mechanical requirements

The drawing specifies cast bronze plus solid lubricant without naming a grade, and separately specifies a maximum load of 100 N/mm², hardness HB 210 to 240, tensile strength above 700 MPa and elongation above 12 per cent.

Table 6 — Matching the stated mechanical envelope to a grade
Stated requirement Value Assessment against published grade data
Maximum load 100 MPa Within the graphite-plugged ceiling of 100 to 120 MPa static. Exceeds every lubricated grade in Table 3, which range from 14 to 60 MPa. This single value effectively specifies a plugged build.
Hardness HB 210 to 240 Matches C86300 at 225 HB. Above C95400 at 150 to 170 HB and marginally above C95500 at 190 to 230 HB.
Tensile strength > 700 MPa Matches C86300 at 758 to 827 MPa. Above C95400 at 517 to 586 MPa. Within the C95500 range at 620 to 655 MPa only at the upper end.
Elongation > 12 % Not published consistently across sources for cast bronzes; must be confirmed against the supplier certificate rather than inferred.
Dry friction factor 0.08 to 0.15 Consistent with a graphite transfer film. Does not discriminate between base alloys.

Conclusion on the reference drawing. The mechanical envelope of hardness HB 210 to 240 with tensile above 700 MPa is consistent with a C86300 manganese bronze base carrying graphite plugs — a documented construction for high-load plugged bushings, not an unusual combination. Aluminium bronze bases (C95400, C95500) are also standard bases for plugged builds, but their published hardness and strength sit below the stated figures, so they would not meet this call-up as drawn. Confirm the grade in writing before production release.

Items requiring written clarification

  1. Base alloy grade. The call-up names no grade. Chemical composition, casting process, plug retention method and cost all follow from this.
  2. Ownership of the hardness figure. HB 210 to 240 may belong to the mating pin rather than to the bushing. If the bushing were held to a conventional HB 80 to 120, several more grades would become selectable.
  3. Plug size, depth and count. The drawing shows a pattern but does not dimension the plugs. Coverage cannot be verified from the drawing alone; the 20 to 30 per cent window in Table 1 must be demonstrated by calculation.
  4. Sliding speed. The drawing carries no speed figure. Without it PV cannot be verified, and the 100 MPa figure cannot be classified as an allowable limit or as a failure load reached at breakage.
  5. Pin material, hardness and finish. The pin is the other half of the friction pair. Pin hardness below approximately 150 HB and surface finish at or below Ra 1.6 are the usual starting assumptions for a copper-alloy bushing.

07Verification before release

Table 7 — Release checklist
# Check Acceptance basis
1 Grade confirmed in writing Named grade with standard reference, not a generic alloy family.
2 PV verified Pressure times sliding speed at or below the PV ceiling in Table 3, with a factor applied.
3 Plug coverage calculated Coverage demonstrated within 20 to 30 per cent, clear of grooves and split lines.
4 Pin hardness and finish specified Not left to the assembly drawing.
5 Hardness and tensile assigned to the correct part Confirms whether the bushing or the pin carries the requirement.
6 Fits resolved Housing bore and pin tolerance classes fixed, not implied by the bushing fit alone.
7 Installation method stated Press or thermal fit; hammer impact on the bushing is not acceptable.

08Frequently asked questions

Why use a self-lubricating bushing in a trolley sheave instead of a plain bronze sleeve?

Because the bushing sits inside the sheave hub, and disassembly requires pressing out the sheave. Scheduled regreasing is impractical at that location, so the lubricant is carried in the component itself.

Is a graphite-plugged bushing suitable for continuous rotation at speed?

Within limits. Published dry sliding speed limits for plugged builds are typically at or below 0.5 m/s, with some sources indicating values up to about 2 m/s under dry conditions. The PV ceiling governs, not speed alone. High-speed continuous service generally calls for an oil-lubricated bronze or a rolling-element bearing instead.

Which bronze grade suits a trolley sheave pin under 100 MPa?

A graphite-plugged build on a high-strength base. C86300 matches a hardness of 210 to 240 HB with tensile above 700 MPa. C95400 and C95500 are standard plugged bases but publish lower hardness and strength than this call-up.

Does the pin material matter?

Yes. The pin is the counterface. Copper-alloy bearings are normally specified against a pin at or below approximately 150 HB with surface finish at or below Ra 1.6. A harder pin raises the risk of galling and reduces service life even when the bushing grade is correct.

How many graphite plugs are needed?

Enough to reach 20 to 30 per cent coverage of the sliding surface, arranged so plugs do not cross a groove or split line and so coverage is continuous through the full arc of oscillation. Plug count alone is not a sufficient specification.

Can the same bushing drawing serve several positions in one crane?

Rarely without qualification. Table 2 shows that acceptable grade changes with shock content, lubrication access and corrosion exposure. Confirm the position first, then confirm the grade against that position.

What does the maximum load figure on a bushing drawing mean in practice?

It is meaningful only with a sliding speed. As drawn, a pressure value without a speed cannot be verified against a PV ceiling, and the figure cannot be classified as an allowable limit or as a failure load reached at breakage.

Source

Material property values are drawn from published standards and supplier technical data for the grades named, including ASTM B438/B438M (SAE 841), ASTM B505 and ASTM B148 (C95400, C95500, C95800), EN 1982 and DIN 825507 for CuAl10Ni5Fe4, and supplier data for C86300. Worked example dimensions were read from drawing J580A210311 and verified against its geometry. Values are design reference ceilings for the duty stated.

Brand neutrality

Alloy designations are standard industry references used for engineering identification. Mention of any grade does not imply supply of that grade. No proprietary product is described or recommended on this page.

Limitation of liability

Allowable pressure, allowable PV and sliding speed figures are reference ceilings for the duty named, not guaranteed performance values. Actual bearing performance depends on alloy composition and manufacturing process, applied radial and axial load, sliding speed, pin hardness and surface finish, temperature, contamination, installation accuracy and service interval. Final material selection, dimensions and operating parameters must be verified against the specific equipment drawings, the OEM requirements and the applicable application calculations.

Copyright

VIIPLUS SOLUTIONS

Metal Bushing (Lubricated Metal) -Self-Lubricating Bushing Materials

Bushings are specialized, self-lubricating metal components widely utilized across various industries due to their durability and low maintenance requirements. Self-lubricating metal bushings are engineered to function without additional lubrication in numerous applications, thereby minimizing maintenance needs. These bushings are available in various series and configurations, such as flanged bushings and split bearings, to meet specific application requirements.

Metal-Polymer Anti-Friction Plain Bearings

Metal-Polymer Composite Self-lubricating Bushing Material

Steel Back + Porous Bronze Sinter + PTFE

Metal-Polymer Plain Bearings Grease Lubricated
Metal-Polymer Plain Bearings Grease Lubricated
Bronze Bearings made of CuSn8 with Lubrication Indents
Bronze Bearings and Bronze Sleeve Bushings made of CuSn8 with Lubrication Indents
Cast Bronze Bushings with Solid Lubricant Inserts
Cast Bronze Bearings with Solid Lubricant Inserts
Bimetal Plain Bearings
Steel + CuPb10Sn10 with indents
Steel Bronze Bushing
Steel Backing and Bronze Overlay
Compare prices and delivery times, then place your order directly online or request a quotation.

lubrication-free Bearing bushing products

Self-lubricating Bushing For High Performance And Low Maintenance